A beneficiation method and low-grade technology, which are applied in the improvement of process efficiency, zinc oxide/zinc hydroxide, calcium/strontium/barium oxide/hydroxide, etc., can solve the problem of low beneficiation recovery rate, low economic value, environmental Pollution and other problems, to achieve high reaction selectivity, reduce energy consumption, and solve the effects of environmental pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0141] In a zinc mine in Yunnan, the zinc content is 11.67%, and the oxidation rate of the original ore is 95.2%. The zinc component in this mine is mainly zinc carbonate.
[0142] Get 300 grams of zinc-containing raw ore, put into 900 milliliters of ammonia-ammonium bicarbonate mixed solution (total ammonia mass concentration 10%, carbonate mass concentration 5%) to carry out stirring and leaching, the leaching temperature is normal temperature, and the stirring time is 2 hours, Then filter, after filtration, the mass concentration of zinc in the liquid is 3.374% (4.2% based on zinc oxide), the mass concentration of carbonate in the liquid is 6.21%, and the increased part is brought in by zinc carbonate in the original ore. According to the inspection data, the recovery rate of soluble zinc in the raw ore during the leaching process was 91.11%, and the recovery rate of total zinc was 86.74%.
[0143] Get the zinc-ammonia complex solution obtained by filtration after 600 milli...
Embodiment 2
[0147] A zinc mine in Chongqing has a zinc content of 12.93% and a raw ore oxidation rate of 94.82%. The zinc in this mine is mainly in the form of zinc silicate.
[0148] Get 300 grams of zinc-containing raw ore, put it into 900 milliliters of ammonia-ammonium bicarbonate mixed solution (total ammonia mass concentration 10%, carbonate mass concentration 6%) for heating and stirring leaching, leaching temperature 50 ° C, stirring time 2 hours , and then filter, after filtration, the mass concentration of zinc in the liquid is 3.681%, and the mass concentration of carbonate in the liquid is 6.34%, and the increased part is brought in by zinc carbonate in the original ore. According to the inspection data, the recovery rate of soluble zinc in the raw ore during the extraction process was 90.07%, and the recovery rate of total zinc was 85.41%.
[0149] Get the zinc-ammonia complex solution obtained by filtration after 600 milliliters of leaching, add 18.98 grams of calcium hydrox...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com