A manufacturing method and the technology of hook and loop fasteners, which are applied in the direction of flame-retardant fibers, fasteners, dry-cleaning fiber products, etc., can solve problems such as unsatisfactory performance requirements, and achieve the effects of accelerating electrostatic dissipation, accelerating dispersion, and reducing static electricity generation Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] A method for manufacturing a water-repellent flame-retardant adhesive tape, the specific steps are as follows:
[0037] Step 1, weaving the nylon Velcro, wherein the weaving process ground yarn arrangement rule is to arrange 1 silver-plated nylon ground yarn every 5 ordinary nylon ground yarns;
[0038] Step 2: Clean the nylon Velcro woven in Step 1. The cleaning equipment is an exhaust dyeing machine, the temperature of the cleaning solution is 80°C, and the cleaning time is 20 minutes;
[0039] Step 3, sequentially carry out flame-retardant finishing and water-repellent finishing on the nylon hook and loop fasteners cleaned in step 2;
[0040] Step 4: Resin finish the nylon hook and loop after flame retardant finishing and water-repellent finishing in step 3. The resin finishing equipment is a gluing machine, the finishing agent temperature is 80°C, and the finishing time is 4 minutes. The resin finishing agent and additives are relatively The weight percentage formu...
Embodiment 2
[0065] A method for manufacturing a water-repellent flame-retardant adhesive tape, the specific steps are as follows:
[0066] Step 1, weaving the nylon Velcro, wherein the arrangement of the bottom yarns in the weaving process is to arrange a silver-plated nylon bottom yarn every 5-8 ordinary nylon bottom yarns;
[0067] Step 2: Clean the nylon Velcro woven in Step 1. The cleaning equipment is an exhaust dyeing machine, the temperature of the cleaning solution is 90°C, and the cleaning time is 30 minutes;
[0068] Step 3, sequentially carry out flame-retardant finishing and water-repellent finishing on the nylon hook and loop fasteners cleaned in step 2;
[0069] Step 4: Carry out resin finishing on the nylon hook and loop after flame-retardant finishing and water-repellent finishing in step 3. The resin finishing equipment is a glue machine, the finishing agent temperature is 100°C, and the finishing time is 6 minutes. The resin finishing agent and additives are relatively Th...
Embodiment 3
[0094] A method for manufacturing a water-repellent flame-retardant adhesive tape, the specific steps are as follows:
[0095] Step 1, weaving the nylon Velcro, wherein the arrangement of the bottom yarns in the weaving process is to arrange a silver-plated nylon bottom yarn every 5-8 ordinary nylon bottom yarns;
[0096] Step 2: Clean the nylon Velcro woven in Step 1. The cleaning equipment is an exhaust dyeing machine, the temperature of the cleaning solution is 85°C, and the cleaning time is 25 minutes;
[0097] Step 3, sequentially carry out flame-retardant finishing and water-repellent finishing on the nylon hook and loop fasteners cleaned in step 2;
[0098] Step 4: Perform resin finishing on the nylon hook and loop after flame-retardant finishing and water-repellent finishing in step 3. The resin finishing equipment is a gluing machine, the finishing agent temperature is 90°C, and the finishing time is 5 minutes. The resin finishing agent and additives are relatively T...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com