A kind of cassiterite flotation combined inhibitor and its application

A combined inhibitor and flotation technology, applied in flotation, solid separation, etc., can solve the problem of lack of high-efficiency and selective inhibitors, and achieve the effect of improving grade, strong effect, and less dosage

Active Publication Date: 2021-10-22
NORTHEASTERN UNIV LIAONING
View PDF9 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] The purpose of the present invention is to provide a cassiterite flotation combination inhibitor to solve the problem of lack of efficient and selective inhibitor for cassiterite flotation separation of calcium-containing minerals in the above-mentioned prior art

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of cassiterite flotation combined inhibitor and its application
  • A kind of cassiterite flotation combined inhibitor and its application
  • A kind of cassiterite flotation combined inhibitor and its application

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0030] 1. Combination inhibitor preparation:

[0031] Mix hydroxycitric acid and citric acid evenly according to the mass ratio of 1:1.

[0032] 2. Raw ore flotation:

[0033] The content of tin in the raw ore is 0.37%. The research results of craft mineralogy show that the main gangue minerals of this mine are quartz, fluorite and calcite. Specific steps are as follows:.

[0034] (1) After the raw ore is crushed, the ore is ground to -0.074mm, accounting for 80%. It is prepared into a pulp in the flotation tank and adjusted to pH 6 with sodium hydroxide and sulfuric acid. Then add 50g / t combined inhibitor, 100g / t The SPA of t is used as a collector, and the 2# oil of 30g / t is used as a foaming agent. After roughing, roughing concentrate and roughing tailings are obtained;

[0035] (2) The rougher tailings after roughing are swept for three times, and 50g / t of SPA is added to each sweep, and the tailings obtained after three sweeps are the final tailings;

[0036] (3) Afte...

Embodiment 2

[0042] 1. Combination inhibitor preparation:

[0043] Mix hydroxycitric acid and citric acid evenly according to the mass ratio of 1:2.

[0044] 2. Raw ore flotation:

[0045] The content of tin in the raw ore is 0.34%. The research results of craft mineralogy show that the main gangue minerals of this mine are quartz, fluorite, calcite and feldspar. Specific steps are as follows:

[0046] (1) After the raw ore is crushed, the ore is ground to -0.074mm to account for 75%. It is prepared into a slurry in the flotation tank and adjusted to pH 8 with sodium hydroxide and sulfuric acid, and then 40g / t of combined inhibitor is added, 80g / t The SPA of t is used as a collector, and the 2# oil of 20g / t is used as a foaming agent, and roughing is carried out to obtain roughing concentrate and roughing tailings;

[0047] (2) The rougher tailings after roughing are swept three times, adding 40g / t of SPA for each sweep, and the tailings obtained after three sweeps are the final tailing...

Embodiment 3

[0054] 1. Combination inhibitor preparation:

[0055] Mix hydroxycitric acid and citric acid evenly according to the mass ratio of 1:1.5.

[0056] 2. Raw ore flotation:

[0057] The content of tin in the raw ore is 0.34%. The research results of craft mineralogy show that the main gangue minerals of this mine are quartz, fluorite, calcite and feldspar. Specific steps are as follows:

[0058] (1) After the raw ore is crushed, the ore is ground to -0.074mm to account for 75%. It is prepared into a slurry in the flotation tank and adjusted to pH 7 with sodium hydroxide and sulfuric acid. Then add 40g / t combined inhibitor, 80g / t The SPA of t is used as a collector, and the 2# oil of 20g / t is used as a foaming agent. After roughing, roughing concentrate and roughing tailings are obtained;

[0059] (2) The rougher tailings after roughing are swept three times, adding 40g / t of SPA for each sweep, and the tailings obtained after three sweeps are the final tailings;

[0060] (3) Afte...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a cassiterite flotation combined inhibitor and its application, and relates to the field of mineral flotation reagents. The combined inhibitor includes hydroxycitric acid (HAC) and lemon with a mass ratio of 1:1 to 1:2 Acid blends are prepared. In the flotation process, 20-50g of combined inhibitors are added to each ton of ore. This combination of inhibitors has the advantages of less dosage, strong effect on calcium-containing minerals, and no pollution to the environment. Effective separation of calcium minerals.

Description

technical field [0001] The invention relates to the field of mineral flotation reagents, in particular to a cassiterite flotation combined inhibitor and its application. Background technique [0002] At present, the gravity separation process is often used to obtain tin concentrate by processing cassiterite minerals, but this process has a better effect when processing tin ore with relatively simple properties. However, with the gradual reduction of easy-to-select ores, the flotation of complex and difficult-to-select tin ores has become the focus of flotation research. However, there are many problems in the flotation of complex and difficult tin ore. The main problem is that the calcium-containing minerals have good buoyancy and are difficult to suppress, which makes it difficult for the grade and recovery rate of tin concentrate to reach the standard. At the same time, traditional inhibitors will make the cassiterite Recycling is also affected to some extent. For comple...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)