A pad material and improved technology, applied in the field of bra pad material and its preparation, can solve the problems of easy aging of sponge, aging of sponge pad, poor elasticity of sponge, etc., achieve good anti-aging performance, wide temperature adaptability range, Effect of improving breathability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A kind of modified bra liner material is prepared according to the following procedures successively:
[0019] Step 1: 1000 grams of granular polyurethane thermoplastic rubber and 150 grams of calcium carbonate were added to the container and kneaded for 4 minutes to mix the two materials evenly;
[0020] Step 2: adding 300 grams of paraffin oil, kneading until all materials are mixed evenly, so that the paraffin oil penetrates into the polyurethane thermoplastic rubber;
[0021] Step 3: Add 50 grams of anti-aging agent RD to mix all materials evenly;
[0022] Step 4: Heat plasticizing through the extruder, then extrude and cut into pellets at the machine head to form 1500 grams of granular bra cushion material. The extruder adopts a single-screw extruder, and the feeding section of the screw The temperature is 165°C, the temperature of the compression section of the screw is 180°C, and the temperature of the melting section of the screw is 185°C. Each component and c...
Embodiment 2
[0024] A kind of bra cushion material is prepared successively according to the following procedures:
[0025] Step 1: 1000 grams of granulated thermoplastic natural rubber and 180 grams of calcium carbonate were added to the container and kneaded for 5 minutes to mix the two materials evenly;
[0026] Step 2: adding 320 grams of naphthenic oil, kneading until all materials are mixed evenly, so that the naphthenic oil penetrates into the thermoplastic natural rubber;
[0027] Step 3: Add 70 grams of anti-aging agent AW to mix all materials evenly;
[0028] Step 4: Heat plasticizing through the extruder, then extrude and pelletize at the machine head to form 1570 grams of granular bra pad material. The extruder adopts a single-screw extruder, and the feeding section of the screw The temperature is 180°C, the temperature of the compression section of the screw is 200°C, and the temperature of the melting section of the screw is 205°C. Each component and content thereof of the ...
Embodiment 3
[0030] A kind of bra cushion material is prepared successively according to the following procedures:
[0031] Step 1: 1000 grams of powdered polyurethane thermoplastic rubber and 190 grams of talcum powder were added into the container and kneaded for 5 minutes to mix the two materials evenly;
[0032] Step 2: adding 340 grams of naphthenic oil, kneading until all materials are mixed evenly, so that the naphthenic oil penetrates into the polyurethane thermoplastic rubber;
[0033] Step 3: Add 60 grams of anti-aging agent AW to mix all materials evenly;
[0034] Step 4: Heat plasticizing through the extruder, then extrude and pelletize at the machine head to form 1590 grams of granular bra pad material. The extruder adopts a single-screw extruder, and the feeding section of the screw The temperature is 168°C, the temperature of the compression section of the screw is 188°C, and the temperature of the melting section of the screw is 198°C. Each component and content thereof o...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com