Special desiccant for box-type transformer substation
A box-type substation and dehumidifier technology, applied in the substation/distribution device shell, gas treatment, membrane technology, etc., can solve the problems of metal parts damage, lower moisture absorption efficiency, easy expansion, etc., to reduce the use cost and moisture absorption efficiency High, large moisture absorption capacity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] A special dehumidifier for a box-type substation, comprising the following components in weight percent: 20% sodium polyacrylate, 7.5% binder, 4% sodium polyaspartate, 1.5% anhydrous copper sulfate, 55% silica gel %, polymethyl acrylate 12%.
[0024] The special hygroscopic agent of preparation present embodiment comprises the following steps:
[0025] 1. Mixing: Pour the ethyl acetate solution of polymethylacrylate into the stirring tank, and the temperature is controlled at room temperature; then, add sodium polyacrylate, sodium polyaspartate, anhydrous copper sulfate, and silica gel according to the proportion ; Finally, add the binder and continue to stir for 2 hours to obtain a well-mixed mixture.
[0026] 2. After the stirring is completed, place the obtained mixture in a vacuum oven, keep the vacuum degree above -98kPa, and dry at 70°C for 3 hours to remove the ethyl acetate solvent.
[0027] 3. Put the dried material obtained in a punching machine, and punch i...
Embodiment 2
[0029] A special dehumidifier for a box-type substation, comprising the following components in weight percent: 15% sodium polyacrylate, 8% binder, 5% sodium polyaspartate, 2% anhydrous copper sulfate, 60% silica gel %, polymethyl acrylate 10%.
[0030] The special hygroscopic agent of preparation present embodiment comprises the following steps:
[0031] 1. Mixing: Pour the ethyl acetate solution of polymethylacrylate into the stirring tank, and the temperature is controlled at room temperature; then, add sodium polyacrylate, sodium polyaspartate, anhydrous copper sulfate, and silica gel according to the proportion ; Finally, add the binder and continue to stir for 3 hours to obtain a well-mixed mixture.
[0032] 2. After the stirring is completed, place the obtained mixture in a vacuum oven, keep the vacuum degree above -98kPa, and dry it at 75°C for 4 hours to remove the ethyl acetate solvent.
[0033] 3. Put the dried material obtained in a punching machine, and punch it...
Embodiment 3
[0035] A special dehumidifier for a box-type substation, comprising the following components in weight percent: 12.5% sodium polyacrylate, 7% binder, 3% sodium polyaspartate, 1.5% anhydrous copper sulfate, 65% silica gel %, polymethyl acrylate 11%.
[0036] The special hygroscopic agent of preparation present embodiment comprises the following steps:
[0037] 1. Mixing: Pour the ethyl acetate solution of polymethylacrylate into the stirring tank, and the temperature is controlled at room temperature; then, add sodium polyacrylate, sodium polyaspartate, anhydrous copper sulfate, and silica gel according to the proportion ; Finally, add the binder and continue to stir for 3 hours to obtain a well-mixed mixture.
[0038] 2. After the stirring is completed, place the obtained mixture in a vacuum oven, keep the vacuum degree above -98kPa, and dry it at 75°C for 5 hours to remove the ethyl acetate solvent.
[0039] 3. Put the dried material obtained in a punching machine, and pu...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com