A production process and aluminized paper technology, applied in papermaking, paper coating, physical treatment of paper, etc., can solve the problems of difficult process control, low production efficiency, high environmental protection requirements, etc., achieve no pollution to the environment, reduce coating costs, and effectively Environmentally friendly effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] Release liner, formulate coated coatings in the following weight ratios:
[0023] Resin: Acetate butyl cellulose resin 15%
[0024] Acetyl cellulose resin 85%
[0026] Diacetone Alcohol 20%
[0027] Ethyl acetate 22%
[0028] Isopropanol 8%
[0029] Resin accounts for 11% by weight of coating;
[0030] Tie coat, formulate the applied coating in the following weight ratios:
[0031] Resin: Acetate butyl cellulose resin 5%
[0032] Acrylic 91%
[0033] Alkyd 4%
[0035] Diacetone Alcohol 20%
[0036] Ethyl acetate 22%
[0037] Isopropanol 10%
[0038] Resin accounts for 13% by weight of coating;
[0039] Use a release layer coating to coat the PET film once (including leveling and drying), and the dry coating amount is 0.6g / m 2 , use the bonding layer coating on the release layer for secondary coating (including leveling and drying), the total ...
Embodiment 2
[0046] For the release layer, prepare a one-coat coating in the following weight ratios:
[0047] Resin: Acetate butyl cellulose resin 20%
[0048] Acetyl cellulose resin 78%
[0049] Acrylic resin 2%
[0051] Diacetone Alcohol 20%
[0052] Ethyl acetate 22%
[0053] Isopropanol 8%
[0054] Resin accounts for 10% by weight of paint
[0055] Tie coat, formulate the applied coating in the following weight ratios:
[0056] Resin: Acetate butyl cellulose resin 5%
[0057] Acrylic 95%
[0058] Solvent: Butanone 48%
[0059] Diacetone Alcohol 20%
[0060] Ethyl acetate 22%
[0061] Isopropanol 10%
[0062] Resin accounts for 11% by weight of coating;
[0063] Then add 1% colorant, 0.3% leveling agent and 0.4% defoamer relative to the weight percentage of the bonding layer coating and mix evenly for later use;
[0064] Coat the PET film once with the above-mentioned release layer coatin...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com