Embodiment 1
[0023] Embodiment 1 A kind of method utilizing the tertiary period solid potash ore reverse flotation method to produce potassium chloride comprises the following steps:
[0024] (1) After the raw ore is crushed to a particle size of less than 1mm by a hammer crusher produced by Wuhan Prospecting Machinery Factory, 750g of raw ore is taken, and 2250g of mother liquor is added to the mixing tank for slurry mixing to obtain 3000g of slurry.
[0025] Wherein the mother liquor refers to the mixed liquor obtained by adding water to the raw material ore according to the weight ratio of raw material ore and water 3:1 to decompose.
[0026] (2) The slurry is sent to the flotation process, and the flotation agent is added to the slurry, wherein the weight ratio of the raw material ore and the flotation agent is 1000:0.05; Flotation was carried out in the process of selection and first-level selection, and the flotation was carried out for 5 minutes. After being filtered by the SS-300 t...
Embodiment 2
[0031] Embodiment 2 A kind of method utilizing the tertiary period solid potash ore reverse flotation method to produce potassium chloride comprises the following steps:
[0032] (1) After the raw ore is crushed by a crusher until the particle size is less than 1mm, 750g of raw ore is taken, and 3000g of mother liquor is added to the stirring tank for slurry mixing to obtain 3750g of slurry.
[0033] Wherein the mother liquor refers to the mixed liquor obtained by adding water to the raw material ore and decomposing it according to the weight ratio of raw material ore and water 3.3:1.
[0034] (2) The slurry is sent to the flotation process, and the flotation agent is added to the slurry, wherein the weight ratio of the raw material ore and the flotation agent is 1000:0.20; Flotation is carried out in the first-level selection process, and the flotation is 5min in total, and 443g of flotation concentrate carnallite (including 90.50% of carnallite), 331g of flotation tailings s...
Embodiment 3
[0039] Embodiment 3 A kind of method that utilizes tertiary solid sylvite reverse flotation method to produce potassium chloride comprises the following steps:
[0040] (1) After the raw ore is crushed by a crusher until the particle size is less than 1mm, 750g of raw ore is taken, and 2625g of mother liquor is added to the stirring tank for slurry mixing to obtain 3375g of slurry.
[0041]Wherein the mother liquor refers to the mixed liquor obtained by adding water to the raw material ore according to the weight ratio of raw material ore and water 3.2:1 to decompose.
[0042] (2) The slurry is sent to the flotation process, and the flotation agent is added to the slurry, wherein the weight ratio of the raw material ore and the flotation agent is 1000:0.13; Flotation is carried out in the first-level selection process, and the flotation is carried out for 5 minutes. After being filtered by a centrifuge, 456g of flotation concentrate carnallite (including 91.01% of carnallite),...