A technology of microcapsules and particle size, applied in botany equipment and methods, fungicides, biocides, etc., can solve the problems of inability to function for a long time and affect the service life of AgO, achieve good thermodynamic stability and maintain antibacterial effect , the effect of simple operation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] The preparation method of AgO microcapsules of this embodiment includes the following steps:
[0028] (1) Take 6g of polystyrene (wall material) and add 60ml of dichloromethane to dissolve to form a polystyrene solution;
[0029] (2) Weigh 0.3 g of AgO nano powder, add it to the polystyrene solution prepared in step (1), add 2% vol of emulsifier Span-80, and ultrasonicate for 30 minutes to form emulsion A;
[0030] (3) Drop the above emulsion A into 500ml of deionized water at a speed of 2ml / min, while stirring with an electric stirrer at a stirring speed of 1000r / min. After the addition is complete, continue to stir and slowly heat to 60°C After 1h, the microcapsules were obtained.
[0031] (4) Filter the above-mentioned microcapsules, then wash them with deionized water, and dry them for later use.
[0032] The AgO microcapsules prepared in this embodiment have a spherical shape, a smooth and uniform surface, a black color, and an average particle size of about 86 μm.
Embodiment 2
[0034] The preparation method of AgO microcapsules of this embodiment includes the following steps:
[0035] (1) Take 6g of polystyrene (wall material) and add 60ml of dichloromethane to dissolve to form a polystyrene solution;
[0036] (2) Weigh 0.6 g of AgO nano powder, add it to the polystyrene solution prepared in step (1), and then add 1% vol of emulsifier Span-80, sonicate it for 30 minutes to form emulsion A;
[0037] (3) Drop the above emulsion A into 500ml of deionized water at a speed of 2ml / min, while stirring with an electric stirrer at a stirring speed of 500r / min. After the addition is complete, continue to stir and slowly heat to 60℃ After 1h, the microcapsules were obtained.
[0038] (4) Filter the above-mentioned microcapsules, then wash them with deionized water, and dry them for later use.
[0039] The AgO microcapsules prepared in this embodiment have a spherical shape, a smooth and uniform surface, a black color, and an average particle size of about 480 μm.