A technology for vacuum insulation panels and core materials, which is applied in heat exchange equipment, mechanical equipment, and pipelines through heat insulation protection, and can solve problems such as difficult displacement, complicated process, and easy breakage of core materials, and achieve easy displacement and preparation Simple method, unbreakable effect
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2013-05-01
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to the field of vacuum heat insulation panels, in particular to a core material for vacuum heat insulation panels, a preparation method and application thereof. Background technique
[0002] At present, the world is facing an energy crisis, and energy conservation and emission reduction have become the focus of worldwide attention. The development of new energy, new technologies and new materials is imperative. As a new type of insulation material, vacuum insulation panel (Vacuum Insulation Panel, referred to as "VIP") has low thermal conductivity and thin thickness. Vacuum insulation panels have great potential for development.
[0003] The composite core material made of powder particles mainly adopts the sol-gel method and the "sandwich structure" method. In the patent document of Chinese Patent No. 200710031196.0 "A Composite Core Material for Vacuum Insulation Panels and Its Preparation Method", a method for preparing a co...
Examples
Embodiment Construction
[0027] The present invention will be described in detail below through specific embodiments.
[0028] A method for preparing a core material for a vacuum insulation panel, the specific steps are as follows:
[0029] Step 1, according to the size of the vacuum insulation panel 200mm×200mm, make a non-woven film bag with one side opening;
[0030] Step 2, according to the core material density is set to 300kg / m 3 1. Mix 120g of loose powder quantitatively with 3g of glass fiber material, fill the non-woven film bag through the opening reserved in step 1, and seal it under normal pressure;
[0031] Step 3, place the non-woven fabric film bag in step 2 flat on a molding machine mold with comparable specifications;
[0032] Step 4, flatten the powder in the non-woven film bag, so that the powder is relatively evenly distributed in the bag;
[0033] Step 5, set the pressure on the molding machine panel to 10000N, and the pressing speed to 24mm / s;
[0034] Step 6, unloading the p...