Loosening agent for regeneration of SCR denitration catalyst and preparation method of agent
A technology of denitration catalyst and regeneration process, which is applied in the field of loosening agent and its preparation to achieve the effect of enhancing active material loading and avoiding damage
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] Weigh 0.5% of the total amount of loosening agent sodium lauryl sulfate, heat it to 70°C on a water bath, and add 2% of the total amount of dimethyl sulfoxide when it is cooled to about 40°C, stir and mix well to obtain Solution A; take 1.5% of the total concentrated H 2 SO 4 Dissolve it in deionized water of the prescribed amount, stir evenly to obtain solution B, and keep it warm at 20°C. Slowly add solution B to solution A, stir while adding until it is evenly mixed, then continue to stir for 10 minutes to obtain a regenerated loose agent with a pH value of 6, and keep the loose agent at 20°C for heat preservation.
[0023] Take the honeycomb-shaped catalyst module that has been blocked and deactivated by the power plant for a long time, and then put it into the loose agent for 20 minutes after simple purge with oil-free dry compressed air. Take it out and rinse the loose agent on the surface of the module with deionized water. .
[0024] The fully cleaned catalys...
Embodiment 2
[0026] Weigh cetyl sodium sulfate accounting for 1% of the total amount of loosening agent, heat it to 70°C on a water bath, and add 3% of the total amount of decyl methyl sulfoxide when it is cooled to about 40°C, and stir well to make the mixture even Obtain solution A; Take the concentrated HNO that accounts for 2% of total amount 3 Dissolve it in deionized water of the prescribed amount, stir evenly to obtain solution B, and keep it warm at 60°C. Slowly add solution B to solution A, stir while adding until it is evenly mixed, and then continue to stir for 10 minutes to obtain a regenerated loose agent with a pH value of 5, and keep the loose agent at 60°C for heat preservation.
[0027] Take the honeycomb-shaped catalyst module that has been blocked and deactivated by the power plant for a long time, and then put it into the loose agent for 20 minutes after simple purge with oil-free dry compressed air. Take it out and rinse the loose agent on the surface of the module wit...
Embodiment 3
[0030] Weigh 2% of the total amount of loosening agent sodium lauryl sulfate and heat it to 70°C on a water bath. When it is cooled to about 40°C, add 3% of the total amount of N-dodecyl-2-pyrrolidone, Stir to make the mixture uniform to obtain solution A; take 2% of the total concentrated H 2 SO 4 Dissolve it in deionized water of the prescribed amount, stir evenly to obtain solution B, and keep it warm at 40°C. Slowly add solution B to solution A, stir while adding until it is evenly mixed, then continue to stir for 10 minutes to obtain a regenerated loose agent with a pH value of 5, and keep the loose agent at 40°C for heat preservation.
[0031] Take the honeycomb-shaped catalyst module that has been blocked and deactivated by the power plant for a long time, and then put it into the loose agent for 20 minutes after simple purge with oil-free dry compressed air. Take it out and rinse the loose agent on the surface of the module with deionized water. .
[0032] The fully...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com