[0023] In concrete implementation, the present invention is realized by the following steps:
[0024] (1) Select Paulownia logs: Choose Paulownia logs with straight main poles, 16 years old, 3m high main poles, no knots, no decay, no skinning, and high-quality Paulownia logs with a veneer area of 125㎡ for a single tree;
[0025] (2) Anti-discoloration and softening treatment of Paulownia logs: Peel the Paulownia logs, put them in a hot water soaking pool, and soak at 70°C for 15 days, and change the water every 3 days;
[0026] (3) Slicing the treated Paulownia logs into Paulownia veneers: Saw the Paulownia logs after anti-discoloration and softening treatment on a band saw machine to make Paulownia squares, and slice the Paulownia squares on a veneer planer to make into 0.6mm thick veneer;
[0027] (4) Paulownia veneer drying: place the paulownia veneer in a place sheltered from the wind and dry until the weight moisture content is 9-10%, cut off the burrs to form a veneer...
Embodiment 2
[0037] In specific implementation, the present invention can also be realized by the following steps:
[0038] (1) Select Paulownia logs: Choose Paulownia logs with straight main poles, 15 years old, 2.6m high main poles, no knots, no decay, no skinning, and high-quality Paulownia logs with a veneer area of 120㎡ for a single tree;
[0039] (2) Anti-discoloration and softening treatment of paulownia logs: Peel the paulownia logs, put them in a hot water soaking pool, and soak them at a temperature of 60°C for 22 days, and change the water every 4 days;
[0040] (3) Slicing the treated Paulownia logs into Paulownia veneers: Saw the Paulownia logs after anti-discoloration and softening treatment on a band saw machine to make Paulownia squares, and slice the Paulownia squares on a veneer planer to make into 0.6mm thick veneer;
[0041] (4) Paulownia veneer drying: place the paulownia veneer in a place sheltered from the wind and dry until the weight moisture content is 9.5%, cu...
Embodiment 3
[0051] The present invention is also realized by the following steps:
[0052] (1) Select Paulownia logs: Choose Paulownia logs with straight main poles, 17 years old, 3m high main poles, no knots, no decay, no skinning, and high-quality Paulownia logs with a single tree with a veneer area of 130㎡;
[0053] (2) Anti-discoloration and softening treatment of paulownia logs: Peel the paulownia logs, put them into a hot water soaking pool, and soak at a temperature of 55°C for 28 days, and change the water every 5 days;
[0054] (3) Slicing the treated Paulownia logs into Paulownia veneers: Saw the Paulownia logs after anti-discoloration and softening treatment on a band saw machine to make Paulownia squares, and slice the Paulownia squares on a veneer planer to make into 0.6mm thick veneer;
[0055] (4) Paulownia veneer drying: place the paulownia veneer in a place sheltered from the wind and dry until the weight moisture content is 10%, cut off the burrs to form a veneer, and...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com