Functionally-modifying method of rubber wood
A rubber wood, modified technology, applied in wood treatment, impregnated wood, wood impregnation, etc., can solve the problems that are not well utilized, rubber wood is easy to deform, wet board is easy to rot, etc., to prevent cracking deformation, waterproof Strong performance and good flame retardancy
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] A method for functional modification of rubber wood, comprising the steps of:
[0037] (1), the rubber wood slab (measured rubber wood specific gravity: 0.65 / cm 3 , with a moisture content of 20%, a thickness of 20mm, and mainly the head section) carry out 2 following impregnation and drying cycles:
[0038]The first impregnation and drying cycle: Put the rubber wood slab into the impregnation tank, vacuumize to -0.06Mpa, keep it for 30 minutes, then inject the impregnation solution, pressurize it to 0.2Mpa, keep it for 8 hours, and finally discharge the impregnation solution;
[0039] Open the impregnation tank, take out the rubber wood slabs, stack the plates and put them in the drying kiln. Under the state of saturated steam, slowly raise the temperature to 160°C, keep it for 8 hours, cool down to 45°C, discharge the saturated steam, and then slowly raise the temperature to 100°C (drying kiln Conventional drying), drying to moisture content ≤ 20%.
[0040] The seco...
Embodiment 2
[0045] A method for functional modification of rubber wood, comprising the steps of:
[0046] (1), the rubber wood slab (measured rubber wood specific gravity: 0.55cm 3 , with a moisture content of 80%, a thickness of 20mm, and mainly the final section) carry out 4 following impregnation and drying cycles:
[0047] The first impregnation and drying cycle: put the rubber wood slab into the impregnation tank, vacuumize to -0.08Mpa, keep it for 20 minutes, then inject the impregnation solution, pressurize it to 0.5Mpa, keep it for 6 hours, and finally discharge the impregnation solution;
[0048] Open the impregnation tank, take out the rubber wood slabs, stack the plates and put them in the drying kiln. Under the state of saturated steam, slowly heat up to 100°C, keep for 24 hours, cool down to 35°C, discharge saturated steam, and then slowly heat up to 80°C (drying kiln Conventional drying), drying to moisture content ≤ 20%.
[0049] The 2nd-4th impregnation and drying cycle:...
Embodiment 3
[0055] A method for functional modification of rubber wood, comprising the steps of:
[0056] (1), the rubber wood slab (measured rubber wood specific gravity: 0.60 / cm 3 , with a moisture content of 50%, a thickness of 20mm, and mainly the head section) carry out 3 following impregnation and drying cycles:
[0057] The first impregnation and drying cycle: put the rubber wood slab into the impregnation tank, vacuumize to -0.07Mpa, keep it for 25 minutes, then inject the impregnation solution, pressurize it to 0.3Mpa, keep it for 7 hours, and finally discharge the impregnation solution;
[0058] Open the impregnation tank, take out the rubber wood slabs, stack the plates and put them in the drying kiln. Under the state of saturated steam, slowly raise the temperature to 120°C, keep it for 15 hours, cool down to 40°C, discharge the saturated steam, and then slowly raise the temperature to 90°C (drying kiln Conventional drying), drying to moisture content ≤ 20%.
[0059] The 2nd...
PUM
Property | Measurement | Unit |
---|---|---|
Thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com