Silent Cork Laminate Floor UV Curing Coating System
A composite floor and ultraviolet light technology, which is applied in the direction of coating, polyester coating, epoxy resin coating, etc., can solve the problems of affecting the indoor environment, insufficient elasticity, poor noise cancellation and mute effect, etc., and achieve the effect of smooth surface effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0057] 1. Preparation of UV elastic putty: Modified epoxy acrylate, difunctional aliphatic urethane acrylate, tripropylene glycol diacrylate TP, isobornyl acrylate IBOA, fumed silica, other additives, photoinitiator Put the reagents into the reaction kettle in sequence according to the mass percentage, heat to 60 ℃ ~ 80 ℃, disperse and stir at high speed for 3 hours.
[0058] 2. Preparation of UV elastic sanding bottom: put modified epoxy acrylate, polyester acrylate, tripropylene glycol diacrylate TP, other additives, talcum powder, and photoinitiator into the reaction kettle in sequence according to mass percentage, and heat To 60 ℃ ~ 80 ℃, high-speed dispersion and stirring for 3 hours.
[0059] 3. Preparation of UV elastic primer: Modified epoxy acrylate, difunctional aliphatic urethane acrylate, polyester acrylate, tripropylene glycol diacrylate TP, hydroxyethyl methacrylate HEMA, other additives, The photoinitiators are put into the reaction kettle in sequence according...
Embodiment 1
[0063] Silent cork composite floor UV curing coating system, the formula mass percentage of its UV elastic putty, UV elastic sanding bottom, UV elastic primer, UV elastic topcoat is as follows:
[0064] The formula mass percentage of UV elastic putty is:
[0065] Modified epoxy acrylate: 45%
[0066] Difunctional Aliphatic Elastomeric Urethane Acrylate: 25%
[0067] Tripropylene glycol diacrylate TP: 8%
[0068] Isobornyl Acrylate IBOA: 8%
[0069] Fumed silica: 8%
[0070] Other additives: 2%
[0071] Photoinitiator: 4%
[0072] The formula mass percent of UV elastic sanding primer is:
[0073] Modified epoxy acrylate: 40%
[0074] Polyester acrylate: 25%
[0075] Tripropylene glycol diacrylate TP: 15%
[0076] Other additives: 2%
[0077] Talc: 14%
[0078] Photoinitiator: 4%
[0079] The formula mass percent of UV elastic primer is:
[0080] Modified epoxy acrylate: 25%
[0081] Difunctional Aliphatic Elastomeric Urethane Acrylate: 45%
[0082] Polyester acry...
Embodiment 2
[0096] Silent cork composite floor UV curing coating system, the formula mass percentage of its UV elastic putty, UV elastic sanding bottom, UV elastic primer, UV elastic topcoat is as follows:
[0097] The formula mass percentage of UV elastic putty is:
[0098] Modified epoxy acrylate: 40%
[0099] Difunctional aliphatic elastic polyurethane acrylate: 20%
[0100] Tripropylene glycol diacrylate TP: 12%
[0101] Isobornyl Acrylate IBOA: 12%
[0102] Fumed silica: 10%
[0103] Other additives: 1.5%
[0104] Photoinitiator: 4.5%
[0105] The formula mass percent of UV elastic sanding primer is:
[0106] Modified epoxy acrylate: 45%
[0107] Polyester acrylate: 20%
[0108] Tripropylene glycol diacrylate TP: 13%
[0109] Other additives: 2.5%
[0110] Talc: 15%
[0111] Photoinitiator: 4.5%
[0112] The formula mass percent of UV elastic primer is:
[0113] Modified epoxy acrylate: 20%
[0114] Difunctional Aliphatic Elastomeric Urethane Acrylate: 44%
[0115] Pol...