Pavement joint filling asphalt material and its preparation method and application

A technology for asphalt material and road petroleum asphalt, which is applied in the field of pavement joint filling asphalt material and its preparation, can solve the problems of poor quality joint filling material failing to meet road performance requirements, being unable to withstand severe cold and low temperature freezing cracking tests, and wasting money. , to achieve the effect of easy operation, saving construction costs and prolonging road life

Active Publication Date: 2018-04-13
山东嘉美泰新材料有限公司
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The application of asphalt joint filling materials in road surface cracks has become a way to repair road surfaces in road maintenance. However, most of the existing technologies use ordinary base asphalt or modified asphalt as joint filling materials, which cannot meet the industry standards. The various indicators required can not withstand the test of freezing and cracking in severe cold and low temperature.
Therefore, every spring, the construction unit repairs the cracks on the asphalt road, but even if it is repaired repeatedly, because the poor-quality filling materials cannot meet the road performance requirements, the rain and snow water has already entered the road base, destroying the road from the inside, resulting in the entire road. The road needs to be repaired, a huge waste of state money

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Pavement joint filling asphalt material and its preparation method and application
  • Pavement joint filling asphalt material and its preparation method and application
  • Pavement joint filling asphalt material and its preparation method and application

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0034] The preparation method of above-mentioned pavement filling asphalt material, comprises the following steps:

[0035] (1) take petroleum asphalt, SBS, rubber powder, compatible stabilizer, asphalt additive and filler by weight;

[0036] (2) Preheat the petroleum asphalt to 180-200°C;

[0037] (3) Put the preheated petroleum asphalt into the premixing tank under the continuous stirring state, and then put the asphalt additive into the premixing tank under the continuous stirring state, and then put SBS and phase into the premixing tank in sequence Soluble type stabilizer, obtain blend;

[0038] (4) Then send the blend into the colloid mill, and the gap between the colloid mill is generally adjusted to 0.2-0.25mm. After grinding, put it into the finished product tank, stir until uniform, and then put rubber powder and filler into the finished product tank in turn, and continue After stirring and reacting for 4-6 hours, it is cooled to obtain the asphalt material for fill...

Embodiment 1

[0043] Pavement filling asphalt, which consists of: 70 parts by weight of 70# petroleum asphalt, 7 parts by weight of SBS, 8 parts by weight of asphalt additive (aromatic content 85%), waste tire rubber powder (60 mesh) of 10 parts by weight, 5 parts by weight of calcium carbonate powder (200 mesh), 0.3 parts by weight of compatible stabilizer (organic solvent content 40%).

[0044] The preparation method and steps of the above-mentioned pavement joint filling asphalt material:

[0045] (1) After weighing the above-mentioned raw materials according to the composition and parts by weight, pass the petroleum asphalt and the asphalt additive through the heat exchange device, and preheat to 180-200°C;

[0046] (2) Put the preheated petroleum asphalt into the premixing tank under the continuous stirring state (300-800 rpm), and then put the asphalt additive into the premixing tank under the continuous stirring state, and then Put SBS and compatible stabilizer into the premixing ta...

Embodiment 2

[0053] Pavement filling asphalt, it consists of: 90# petroleum asphalt of 55 parts by weight, SBS of 10 parts by weight, asphalt additive (aromatic hydrocarbon content 90%) of 30 parts by weight, waste tire rubber powder (80 orders) of 15 parts by weight and 0.25 parts by weight of compatible stabilizer (organic solvent content 50%).

[0054] The preparation method and steps of the above-mentioned pavement joint filling asphalt material:

[0055] (1) After weighing the above-mentioned raw materials according to the composition and parts by weight, pass the petroleum asphalt and the asphalt additive through the heat exchange device, and preheat to 180-200°C;

[0056] (2) Put the preheated petroleum asphalt into the premixing tank under the continuous stirring state (300-800 rpm), and then put the asphalt additive into the premixing tank under the continuous stirring state, and then Put SBS and compatible stabilizer into the premixing tank in turn to obtain the blend;

[0057]...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
sizeaaaaaaaaaa
Login to View More

Abstract

The invention relates to a pavement joint filling asphalt material and a preparation method and application thereof, belonging to the technical field of road paving special materials. It solves the problem that the joint filling asphalt technology for roads in low temperature and severe cold areas in the prior art is not up to standard, thereby prolonging the life of the road surface and reducing the cost of road maintenance. The composition and parts by weight of the pavement joint filling asphalt material of the present invention are: 40-70 parts by weight of road petroleum asphalt, 7-15 parts by weight of SBS, 10-20 parts by weight of rubber powder, and 0.2-0.4 parts by weight of compatible type Stabilizer, 8-40 parts by weight of asphalt additive and 0-8 parts by weight of filler. The pavement joint filling asphalt has high elasticity and toughness, stable low temperature resistance, stretching can reach 3 100% cycles at ‑30 ° C, no flow at +80 ° C high temperature, fully achieve low temperature without brittle cracking, high temperature The concept of non-flowing joint-filling asphalt can meet the needs of repairing cracks in asphalt and cement roads, and is suitable for use in different climate regions across the country.

Description

technical field [0001] The invention relates to a pavement joint filling asphalt material and a preparation method and application thereof, belonging to the technical field of special materials for paving roads, and applicable to different domestic and international climate zones. Background technique [0002] In the later stage of asphalt road construction, due to the alternation of high temperature in summer and severe cold in winter, coupled with the penetration of rain, snow and ice, there will be horizontal and vertical cracks and cracks on the road surface. The life of the pavement is seriously threatened. The application of asphalt joint filling materials in road surface cracks has become a way to repair road surfaces in road maintenance. However, most of the existing technologies use ordinary base asphalt or modified asphalt as joint filling materials, which cannot meet the industry standards. The various indicators required cannot withstand the test of freezing and...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C08L95/00C08L53/02C08L21/02C08K3/26C08K3/34
Inventor 林雨冬
Owner 山东嘉美泰新材料有限公司