Embodiment 1
[0027] Sizing dyed black denim yarn
[0028] (1) Configure paint color paste 1, the composition and percentage of paint color paste are as follows:
[0029] Coating carbon black 50%
[0030] Cationic binder PDY (Changzhou Hansi Chemical Co., Ltd.) 30%
[0031] Polyvinylpyrrolidone 20%
[0032] After the above ingredients are evenly mixed, adjust the pH to 6.5 with citric acid.
[0033] (2) Get the paint color paste 1 obtained in step (1) and configure the dyeing solution as follows:
[0034]
[0035]
[0036] After mixing, adjust the pH value to 7-8 with sodium carbonate;
[0037] (3) After the sizing is first wetted with hot water, padding is carried out through the dyeing solution of step (2), and the excess rate is 95%, dried by an 80°C drying cylinder, steamed (105°C, 60s), Then bake in a baking oven at a temperature of 120°C for 4 minutes;
[0038] (4) Water washing (1 soaping → 1 hot washing → 2 cold washings → drying).
[0039] The dyed black denim yarn has...
Embodiment 2
[0044] Distressed dark blue denim over dyed with indigo denim yarn
[0045] (1) Configure paint color paste 2, the composition and percentage of the paint color paste are as follows:
[0046] Coating carbon black 60%
[0047] Cationic binder PDY (Changzhou Hansi Chemical Co., Ltd.) 30%
[0048] CMC 10%
[0049] After the above ingredients are evenly mixed, adjust the pH to 6 with citric acid.
[0050] (2) Get the paint color paste 2 that step (1) obtains and configure the dyeing solution as follows:
[0051]
[0052] After mixing, adjust the pH to 7.5 with sodium bicarbonate;
[0053] (3) After the indigo yarn is wetted with hot water, the dyeing solution of step (2) is used for padding, the excess rate is 100%, dried by a 90°C dryer, and steamed (110°C, 60s) , and then baked in a baking oven at a temperature of 125°C for 4 minutes;
[0054] (4) Water washing (1 soaping → 1 hot washing → 1 cold washing → 1 hot washing → 1 cold washing → drying).
[0055]The dyed blac...
Embodiment 3
[0060] Using white denim woven fabric (white cow) (320g / m 2 ) dyed yellow
[0061] (1) Configure the paint color paste 3, the composition and percentage of the paint color paste are as follows:
[0062] Paint Chrome Yellow 60%
[0063] Cationic binder PDY (Changzhou Hansi Chemical Co., Ltd.) 25%
[0064] Polypropylene Glycol 15%
[0065] After the above ingredients were uniformly mixed, the pH was adjusted to 7 with acetic acid.
[0066] (2) Get the paint color paste 3 that obtains in step (1) and configure the dyeing solution as follows:
[0067]
[0068] After mixing, adjust the pH to 8 with sodium bicarbonate;
[0069] (3) After wetting the white cattle with hot water, padding with the dyeing solution in step (2), the excess rate is 105%, drying in a drying cylinder at 100°C, steaming (102°C, 90s), Then bake in a baking oven at a temperature of 120°C for 4 minutes;
[0070] (4) Water washing (1 soaping → 1 hot washing → 1 cold washing → drying).
[0071] The dyed...
PUM
Property | Measurement | Unit |
---|---|---|
color fastness | aaaaa | aaaaa |
color fastness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com