A kind of heat reflective coating cloth
A technology of heat reflective coating and coated cloth, which is applied in the field of applied chemistry, can solve the problems of poor decoration, poor reflection effect, and easy falling off of the reflective layer, achieve good stability and weather resistance, reduce aging rate, and reduce energy consumption The effect of consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0038] According to the present invention, the preparation method of the second coating slurry in the coating cloth may include: mixing and stirring each component in the top coating composition, and then filtering the filtrate obtained is the coating slurry. Ply the second coating slurry.
[0039] According to a preferred embodiment of the present invention, the preparation method of the second coating slurry of the coated cloth may include: putting water into a dispersion tank, and sequentially adding a dispersant at a speed of 300-500 rpm , titanium dioxide, near-infrared reflective pigment and defoamer, increase the speed to 1500 rpm, disperse at high speed for 1.5-2 hours, use a scraper fineness meter to detect the fineness below 30 microns, and lower the speed to 300 rpm minutes, then add anionic emulsion, leveling agent and anti-sedimentation agent, stir evenly, and then filter, and the filtrate obtained by filtering is the second coating slurry for the coated cloth.
...
Embodiment 1
[0046] 40 parts by weight of alcohol are dropped into the dispersing tank, and 3.9 parts by weight of dispersant (Deqian Chemical Co., Ltd., brand NUOSPERSE FX 600) and 56 parts by weight of large particles with an average particle diameter of 0.8 micron are dropped into successively at a speed of 500 rpm. Diameter rutile titanium dioxide (purchased from Shanghai Baitu High-tech Material Technology Co., Ltd., brand BR80), dispersed for 1.5 hours, and when the fineness was detected by a scraper fineness meter to below 30 microns, the speed was reduced to 300 rpm, and then added 100 parts by weight of pure acrylate self-crosslinking anionic emulsion (purchased from Shanghai Baolijia Chemical Co., Ltd., brand BLJ-718), 0.9 parts by weight of leveling agent (purchased from Deqian Chemical Co., Ltd., brand SLIP-AYD FS444), 1.5 Parts by weight of anti-settling agent (purchased from German BYK Chemical Co., Ltd., brand BYK420) and 1.6 parts by weight of foaming agent (purchased from B...
Embodiment 2
[0050] 20 parts by weight of alcohol are dropped into the dispersion tank, and 2.4 parts by weight of dispersant (purchased from Deqian Chemical Co., Ltd., brand NUOSPERSE FX 600) and a large particle size of 1.3 microns are dropped into successively at a speed of 500 rpm. Rutile type titanium dioxide (purchased from Shanghai Baitu High-tech Material Technology Co., Ltd., brand BR80) 50 parts by weight, dispersed for 1.5 hours, and when the fineness was detected by a scraper fineness meter to below 30 microns, the rotating speed was reduced to 300 rpm, Then add 100 parts by weight of pure acrylate self-crosslinking anionic emulsion (purchased from Shanghai Baolijia Chemical Co., Ltd., brand BLJ-718), and 0.8 parts by weight of leveling agent (purchased from Deqian Chemical Co., Ltd., brand SLIP-AYD FS444) , 1.8 parts by weight of anti-settling agent and 3.0 parts by weight of foaming agent (purchased from Bengbu Xin'ao Rubber and Plastic Technology Co., Ltd., brand WBA), stirre...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| particle size | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |