Method using ammonium exchange method to prepare low-methoxyl pectin
A technology of low-ester pectin and high-ester pectin, applied in the field of food processing, can solve the problems of high production cost, high equipment requirements, and high requirements for supporting auxiliary equipment, and achieve low production cost, mild reaction conditions, and simple process flow Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] 1) Add 3g of pectin powder to a 100ml Erlenmeyer flask, then add distilled water to 100ml, shake to completely dissolve the pectin.
[0026] 2) When the pectin is completely dissolved, add 7ml of 25g / L ammonium acetate solution, and stir at 40°C for 24h.
[0027] 3) Use hydrochloric acid to adjust the pH of the solution to 2, then add 2 times the volume of absolute ethanol, stir evenly, filter to obtain pectin precipitate, dry with hot air at 40°C to constant weight, and pulverize to obtain low-ester pectin.
[0028] The degree of esterification of low-ester pectin was determined to be 43% by titration. After the sample was dried, the composition of the sample was analyzed by infrared spectroscopy and compared with a low-ester pectin standard, such as figure 1 and figure 2 . The results showed that the absorption peaks of the samples were basically consistent with those of the standard substance, indicating that this method only reduced the degree of esterification ...
Embodiment 2
[0030] 1) Add 2g of pectin powder into a 100ml Erlenmeyer flask, then add distilled water to 100ml, shake to completely dissolve the pectin.
[0031] 2) When the pectin is completely dissolved, add 4.5ml of 20g / L ammonium acetate solution, and stir at 70°C for 1h.
[0032] 3) Use hydrochloric acid to adjust the pH of the solution to 1, then add 3 times the volume of absolute ethanol, stir evenly, filter to obtain pectin precipitate, dry with hot air at 50°C to constant weight, and pulverize to obtain low-ester pectin.
[0033] The esterification degree of gained low-ester pectin is 49%, and infrared spectrum sees image 3 .
Embodiment 3
[0035] 1) Add 4g of pectin powder to a 100ml Erlenmeyer flask, then add distilled water to 100ml, shake to completely dissolve the pectin.
[0036] 2) When the pectin is completely dissolved, add 6ml of 30g / L ammonium acetate solution, and stir at 50°C for 12h.
[0037] 3) Use hydrochloric acid to adjust the pH of the solution to 3, then add 5 times the volume of absolute ethanol, stir evenly, filter to obtain pectin precipitate, dry with hot air at 60°C to constant weight, and pulverize to obtain low-ester pectin.
[0038] The esterification degree of gained low-ester pectin is 45%, and infrared spectrum sees Figure 4 .
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology