Low-cost wall brick
A low-cost, wall brick technology, applied in the field of building materials, can solve the problems of environmental pollution, increased production cost, heavy weight, etc., to improve fluidity and adhesion, improve high strength and wear resistance, and reduce production costs. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] A low-cost wall brick described in this embodiment includes the following raw materials: slag: 25 parts by weight, construction dregs: 40 parts by weight, grinding wheel ash: 26 parts by weight, straw: 4 parts by weight, limestone: 8 parts by weight, Vermiculite: 1 part by weight, river water: 85 parts.
[0037] The preparation method of above-mentioned low-cost wall brick, comprises the following steps:
[0038] (1) The slag is crushed by the three-stage crushing method of jaw crushing, hammer crushing and squirrel cage crushing, and the particle size after crushing is controlled at 1mm;
[0039] (2) Mix the grinding wheel ash with the slag particles after step (1), seal and heat, keep the temperature at 260°C, the pressure at 58KPa, and the time for 4h;
[0040] (3) Crush the limestone into 1800 mesh fine powder;
[0041](4) The three-stage crushing method of jaw crushing, hammer crushing, and squirrel cage crushing is used to crush the construction waste, and the p...
Embodiment 2
[0051] A low-cost wall brick described in this embodiment includes the following raw materials: slag: 20 parts by weight, construction dregs: 45 parts by weight, grinding wheel ash: 25 parts by weight, straw: 5 parts by weight, limestone: 5 parts by weight, Vermiculite: 2 parts by weight, river water: 80 parts.
[0052] The preparation method of above-mentioned low-cost wall brick, comprises the following steps:
[0053] (1) The slag is crushed by the three-stage crushing method of jaw crushing, hammer crushing and squirrel cage crushing, and the particle size after crushing is controlled at 2mm;
[0054] (2) Mix the grinding wheel ash with the slag particles after step (1), seal and heat, keep the temperature at 250°C, the pressure at 60KPa, and the time for 3h;
[0055] (3) Crush the limestone into 2000 mesh fine powder;
[0056] (4) The three-stage crushing method of jaw crushing, hammer crushing, and squirrel cage crushing is used to crush the construction waste, and the...
Embodiment 3
[0066] A low-cost wall brick described in this embodiment includes the following raw materials: slag: 30 parts by weight, construction dregs: 35 parts by weight, grinding wheel ash: 28 parts by weight, straw: 3 parts by weight, limestone: 10 parts by weight, Vermiculite: 1 part by weight, river water: 90 parts.
[0067] The preparation method of above-mentioned low-cost wall brick, comprises the following steps:
[0068] (1) The slag is crushed by the three-stage crushing method of jaw crushing, hammer crushing and squirrel cage crushing, and the particle size after crushing is controlled at 1mm;
[0069] (2) Mix the grinding wheel ash with the slag particles after step (1), seal and heat, keep the temperature at 275°C, the pressure at 60KPa, and the time for 5h;
[0070] (3) Crush the limestone into 1500 mesh fine powder;
[0071] (4) The three-stage crushing method of jaw crushing, hammer crushing, and squirrel cage crushing is used to crush the construction waste, and the...
PUM
Property | Measurement | Unit |
---|---|---|
size | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com