Preparation method and application of modified waterborne polyurethane antibacterial coating
A water-based polyurethane and antibacterial coating technology, which is applied in polyurea/polyurethane coatings, coatings, antifouling/underwater coatings, etc., can solve the problems of reducing the volatilization degree of lemon eucalyptus essential oil, volatilization and instability of lemon eucalyptus essential oil
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] Embodiment 1 lemon eucalyptus essential oil / g-C 3 N 4 Preparation and Properties of Composite Modified Waterborne Polyurethane Coating Film
[0025] 1 Experimental materials
[0026] Urea; AR; Sinopharm Chemical Reagent Co., Ltd.
[0027] Absolute ethanol; AR; Sinopharm Chemical Reagent Co., Ltd.
[0028] Essential oil of lemon eucalyptus; AR; French florihana essential oil.
[0029] Water-based polyurethane; Qingdao Jient Technology Co., Ltd., Shandong Province.
[0030] 2 Experimental methods
[0031] 1) g-C 3 N 4 Absorb lemon eucalyptus essential oil
[0032] ①Weigh 160 μL of 100% (V / V) essential oil of lemon eucalyptus, add 1440 μL of absolute ethanol to dissolve and make 10% (V / V) essential oil of lemon eucalyptus.
[0033] ② Weigh 5 parts of 0.125g-C 3 N 4 Into a 5mL centrifuge tube, according to the mass ratio of 1:1, 1:2, 1:3, 1:4, 1:5, add different volumes of 10% lemon eucalyptus essential oil respectively, and seal and stir at 40°C for 24h to make ...
Embodiment 2
[0064] The research on the anti-staphylococcus aureus biofilm effect on the iron sheet of the modified waterborne polyurethane coating film prepared by embodiment 2
[0065] 1 Experimental materials
[0066] ①Modified water-based polyurethane
[0067] ② Staphylococcus aureus
[0068] 2 Experimental methods
[0069] 1) Preparation of bacterial solution
[0070] Directly take the strains inoculated in the test tube of nutrient broth medium, after culturing Staphylococcus aureus for 48 hours, mix it with a shaker, and dilute it 10 times with 0.03mol / L phosphate buffer solution 10 times (about 1000 times) 5 cfu / mL).
[0071] 2) Preparation of lemon eucalyptus essential oil / g-C 3 N 4 Composite material modified waterborne polyurethane coating film
[0072] With reference to the above-mentioned embodiment 1, the lemon eucalyptus essential oil / g-C with different adsorption ratios prepared by using a 10mm×10mm metal iron sheet as the sample base plate 3 N 4 The composite mate...
Embodiment 3
[0085] The research on the anti-staphylococcus aureus biofilm effect on the glass sheet of the modified water-based polyurethane coating film prepared by embodiment 3
[0086] 1 Experimental materials
[0087] ①Modified water-based polyurethane
[0088] ② Staphylococcus aureus
[0089] 2 Experimental methods
[0090] 1) Preparation of bacterial solution
[0091] Directly take the strains inoculated in the test tube of nutrient broth medium, after culturing Staphylococcus aureus for 48 hours, mix it with a shaker, and dilute it 10 times with 0.03mol / L phosphate buffer solution 10 times (about 1000 times) 5 cfu / mL).
[0092] 2) Preparation of lemon eucalyptus essential oil / g-C 3 N 4 Composite material modified waterborne polyurethane coating film
[0093] With reference to the above-mentioned embodiment 1, the lemon eucalyptus essential oil / g-C of different adsorption ratios will be prepared with a 10mm × 10mm glass sheet as the sample bottom plate 3 N 4 The composite mat...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com