A kind of preparation method of waterproof art paint
A production method and pigment technology, applied in the field of painting supplies, can solve the problems of the pigment flowing to other places, the pigment adhering to the clothes, the pigment being cracked or granular, etc., so as to improve the anti-oxidation performance, improve the adhesion, and improve the color and luster. long lasting effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0013] A kind of preparation method of waterproof art paint that the present invention proposes, comprises the following steps:
[0014] S1: Put the epoxy resin in a pulverizer to pulverize it, then put it in a smelter and melt it for 4 minutes to obtain a resin liquid, including 50 parts of epoxy resin, 25 parts of mica powder, and 8 parts of nano-silica;
[0015] S2: Dissolve corresponding parts by weight of neopentyl polyol ester, glycerin, silicone oil, dibutyl phthalate and polyethylene glycol in ethanol solution, and stir at a speed of 300r / min for 5min to obtain mixed solution A , including 7 parts of neopentyl polyol ester, 4 parts of glycerin, 6 parts of silicone oil, 4 parts of dibutyl phthalate, and 4 parts of polyethylene glycol;
[0016] S3: Add the resin solution prepared in step S1 to the mixed solution A, and stir at a speed of 300r / min for 10min, then add tris(2,4-di-tert-butylphenyl) phosphite, di-tert-butyl Hydroxytoluene, pigment powder, dispersant, anti-s...
Embodiment 2
[0019] A kind of preparation method of waterproof art paint that the present invention proposes, comprises the following steps:
[0020] S1: Put the epoxy resin in a pulverizer to pulverize it, and then put it in a smelting machine for smelting for 5 minutes to obtain a resin liquid, including 60 parts of epoxy resin, 30 parts of mica powder, and 5 parts of nano-silica;
[0021] S2: Dissolve corresponding parts by weight of neopentyl polyol ester, glycerin, silicone oil, dibutyl phthalate and polyethylene glycol in ethanol solution, and stir at a speed of 200r / min for 10min to obtain mixed solution A , wherein 10 parts of neopentyl polyol ester, 6 parts of glycerin, 6 parts of silicone oil, 2 parts of dibutyl phthalate, 4 parts of polyethylene glycol;
[0022] S3: Add the resin solution prepared in step S1 to the mixed solution A, and stir at a speed of 200r / min for 20min, then add tris(2,4-di-tert-butylphenyl) phosphite, di-tert-butyl Hydroxytoluene, pigment powder, dispersa...
Embodiment 3
[0025] A kind of preparation method of waterproof art paint that the present invention proposes, comprises the following steps:
[0026] S1: Put the epoxy resin in a pulverizer to pulverize it, and then put it in a smelter to melt for 4 minutes to obtain a resin liquid, including 30 parts of epoxy resin, 30 parts of mica powder, and 8 parts of nano-silica;
[0027] S2: Dissolve corresponding parts by weight of neopentyl polyol ester, glycerin, silicone oil, dibutyl phthalate and polyethylene glycol in ethanol solution, and stir at a speed of 300r / min for 10min to obtain mixed solution A , wherein, 10 parts of neopentyl polyol ester, 4 parts of glycerin, 4 parts of silicone oil, 8 parts of dibutyl phthalate, 6 parts of polyethylene glycol;
[0028] S3: Add the resin solution prepared in step S1 to the mixed solution A, and stir at a speed of 300r / min for 20min, then add tris(2,4-di-tert-butylphenyl) phosphite, di-tert-butyl Hydroxytoluene, pigment powder, dispersant, anti-sedi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com