Unlock instant, AI-driven research and patent intelligence for your innovation.

Manufacturing method for two-layer two-color flannel imitation snowflake two-color split leather

A production method and a technology for two-layer leather, which are applied in leather manufacturing, leather drying, leather surface mechanical treatment, etc., can solve the problem of flannel having no two-color effect, etc., and achieve good friction and fading resistance, good elasticity, and smooth texture. Effect

Active Publication Date: 2018-01-19
漳州香洲皮革有限公司
View PDF3 Cites 4 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] But flannel has no two-color effect, and there is no example of flannel imitating two-color snowflakes in China at present. Therefore, the applicant provides a method for making two-layer two-color flannel imitating snowflake two-color two-layer leather

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Manufacturing method for two-layer two-color flannel imitation snowflake two-color split leather

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0048] The manufacturing method of two-layer two-color flannel imitation snowflake two-color two-layer leather comprises the following steps:

[0049] Step 1, rehumidification: take the processed and dyed two-layer leather and put it in the drum, add 200% of 50°C water, 0.5% sodium carbonate, and 0.5% of LIPIDOL DG to the drum according to the weight of the leather 118 degreasing agent and 0.3% oxalic acid, rotate for 60 minutes, drain the drum, then add water to wash and drain;

[0050] Step 2, retanning: add 50% water and 2% glutaraldehyde according to the weight of the leather to the drum, rotate for 20 minutes, add 4% chrome powder and 0.5% formic acid, and rotate for 90 minutes;

[0051] Step 3, alkali extraction: add 1.2% sodium formate and 0.8% sodium acetate according to the weight of leather to the drum, rotate for 60 minutes, drain the drum, then add water to wash and drain;

[0052] Step 4, neutralization: add 50% water, 1% sodium formate and 1% TJ-R819 neutralizin...

Embodiment 2

[0061] The manufacturing method of two-layer two-color flannel imitation snowflake two-color two-layer leather comprises the following steps:

[0062] Step 1, rehumidification: take the processed and dyed two-layer leather and put it in the drum, add 150% of 40°C water, 0.3% sodium carbonate, and 0.3% of LIPIDOL DG to the drum according to the weight of the leather 118 degreaser and 0.1% oxalic acid, rotate for 80 minutes, drain the drum, then add water to wash and drain;

[0063] Step 2, retanning: add 40% water and 1% glutaraldehyde according to the weight of the leather to the drum, rotate for 30 minutes, add 2% chrome powder and 0.2% formic acid, and rotate for 110 minutes;

[0064] Step 3, alkali extraction: add 0.8% sodium formate and 0.5% sodium acetate according to the weight of leather to the drum, rotate for 90 minutes, drain the drum, then add water to wash and drain;

[0065] Step 4, neutralization: add 40% water, 0.5% sodium formate and 0.6% TJ-R819 neutralizing ...

Embodiment 3

[0074] The manufacturing method of two-layer two-color flannel imitation snowflake two-color two-layer leather comprises the following steps:

[0075] Step 1, rehumidification: take the processed and dyed two-layer leather and put it in the drum, add 300% of 60°C water, 1% sodium carbonate, and 1% of LIPIDOL DG to the drum according to the weight of the leather 118 degreasing agent and 0.8% oxalic acid, rotate for 50 minutes, drain the drum, then add water to wash and drain;

[0076] Step 2, retanning: add 60% water and 5% glutaraldehyde according to the weight of leather to the drum, rotate for 15 minutes, add 8% chrome powder and 1% formic acid, and rotate for 80 minutes;

[0077] Step 3, alkali extraction: add 2% sodium formate and 1.6% sodium acetate according to the weight of the leather to the drum, rotate for 50 minutes, drain the drum, then add water to wash and drain;

[0078] Step 4, neutralization: add 60% water, 1.3% sodium formate and 1.2% TJ-R819 neutralizing ag...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a manufacturing method for two-layer two-color flannel imitation snowflake two-color split leather and belongs to the technical field of leather. The manufacturing method forthe two-layer two-color flannel imitation snowflake two-color split leather comprises the following steps that the processed and dyed split leather is taken, rewetting, retanning, leather basifying, neutralizing, fatliquoring, acid fixing, color fixing, dyeing, drying, drum milling and leather grinding are sequentially performed, and the two-layer two-color flannel imitation snowflake two-color split leather is obtained. The manufactured two-layer two-color flannel imitation snowflake two-color split leather not only has the excellent tensile property, the good abrasion and fading resistance and the good waterproofness, but also has the obvious two-color appearance, the soft hand feel, the smooth texture, good skin friendliness and good elasticity.

Description

technical field [0001] The invention belongs to the technical field of leather, in particular to a method for making two-layer double-color flannel imitation snowflake double-color double-layer leather. Background technique [0002] The color of flannel is pure and generous, which can be divided into light gray, medium gray and dark gray. The weight of flannel is high, the plush is relatively fine and dense, the fabric is thick, and it has good warmth retention. The surface of flannel has a plump and fine layer. It is covered with fluff, does not reveal texture, feels soft and flat, and has a slightly thinner body bone than Melton. After milling and fluffing, the hand feels full and the suede is fine. [0003] But flannel does not have two-color effect, and there is no example of flannel imitating snowflake two-color at present in China, therefore, the applicant provides a kind of manufacturing method of two-layer two-color flannel imitating snowflake two-color two-color le...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More