A labeling machine and plastic bottle technology, which is applied in the direction of rosin adhesive, adhesive type, ester copolymer adhesive, etc., can solve the problems of unsuitable high-speed automatic labeling, affecting the aesthetics of beer, and poor affinity , to achieve the effects of small temperature difference, low cost, and smooth labeling
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] Embodiment one: the preparation method of plastic bottle environmental protection label adhesive for automatic labeling machine, the steps are:
[0024] (1), 150 kg of deionized water is added to the reaction vessel, then 6 kg of OP-10 is added, and stirred at high speed for 10 minutes;
[0025] (2), add 12 kilograms of rosin, 30 kilograms of methacrylic acid, 35 kilograms of methyl methacrylate, 40 kilograms of ethyl acrylate, and 120 kilograms of butyl acrylate in the above-mentioned reaction vessel in sequence, and continue high-speed stirring for 60-120 minutes;
[0026] (3), dissolve 2 kilograms of ammonium persulfate with 10 kilograms of deionized water, add 9.6 kilograms in the above-mentioned reaction vessel, continue to stir for 10 minutes and make pre-emulsified reaction solution A;
[0027] (4), add 350 kg of deionized water to another reactor, add 80 kg of polyvinyl alcohol, heat up to 85-90°C, keep warm for 2 hours, and cool down to 82±2°C;
[0028] (5), u...
Embodiment 2
[0031] Embodiment two: the preparation method of plastic bottle environmental protection label adhesive for automatic labeling machine, the steps are:
[0032] (1), add 150 kilograms of deionized water to the reaction vessel, then add 6 kilograms of OS, and stir at high speed for 10 minutes;
[0033] (2), add 15 kilograms of rosin, 35 kilograms of methacrylic acid, 35 kilograms of methyl methacrylate, 50 kilograms of ethyl acrylate, and 100 kilograms of butyl acrylate in the above-mentioned reaction vessel in sequence, and continue high-speed stirring for 60-120 minutes;
[0034] (3), dissolve 2 kilograms of ammonium persulfate with 10 kilograms of deionized water, add 9.6 kilograms in the above-mentioned reaction vessel, continue to stir for 10 minutes and make pre-emulsified reaction solution A;
[0035] (4) Add 350 kg of deionized water to another reactor, add 100 kg of polyvinyl alcohol, heat up to 85-90°C, keep warm for 2 hours, and cool down to 82±2°C;
[0036] (5), und...
Embodiment 3
[0039] Embodiment three: the preparation method of plastic bottle environmental protection label adhesive for automatic labeling machine, the steps are:
[0040] (1), 150 kg of deionized water is added to the reaction vessel, then 6 kg of OP-10 is added, and stirred at high speed for 10 minutes;
[0041] (2), add 50 kilograms of rosin, 100 kilograms of methacrylic acid, 60 kilograms of methyl methacrylate, 800 kilograms of ethyl acrylate, and 200 kilograms of butyl acrylate in the above-mentioned reaction vessel in sequence, and continue high-speed stirring for 60-120 minutes;
[0042] (3), dissolve 10 kilograms of ammonium persulfate with 10 kilograms of deionized water, add 9.6 kilograms in the above-mentioned reaction vessel, continue to stir for 10 minutes and make pre-emulsified reaction solution A;
[0043] (4), add 400 kg of deionized water to another reactor, add 200 kg of polyvinyl alcohol, heat up to 85-90°C, keep warm for 2 hours, and cool down to 82±2°C;
[0044] ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com