A technology of ruthenium dioxide and ovalbumin, applied to wave energy or particle radiation treatment materials, medical preparations with non-active ingredients, medical preparations containing active ingredients, etc., can solve the problems of cancer immunotherapy that have not been reported , to achieve good photodynamic effect, inhibit remote cells, and prevent tumor recurrence
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation Embodiment 1
[0026] 1) Weigh 0.4g ruthenium trichloride hydrate, add 10mL distilled water, stir to dissolve completely, and obtain ruthenium trichloride hydrate solution;
[0027] 2) Add ammonia water to the hydrated ruthenium trichloride solution to adjust the pH of the solution to 9, and react for 30 minutes to obtain a solution with black precipitates;
[0028] 3) Centrifuge the solution in step 2) with a centrifuge at a speed of 10,000r / min for 10 minutes; the precipitate obtained by centrifugation is washed twice with water, and then centrifuged to obtain a black precipitate;
[0029] 4) Heating the precipitate obtained in step 3) in nitrogen gas at a heating temperature of 200°C for 2 hours to obtain nano-scale ruthenium dioxide;
[0030] 5) Take 0.1 g of the ruthenium dioxide obtained in step 4) and add 0.1 g of ovalbumin into 100 mL of water and sonicate for 30 minutes to obtain a ruthenium dioxide composite ovalbumin nanomaterial.
Embodiment 2
[0032] Preparation of ruthenium dioxide composite ovalbumin nanomaterials:
[0033] 1) Weigh 0.4g ruthenium trichloride hydrate, add 10mL distilled water, stir to dissolve completely, and obtain ruthenium trichloride hydrate solution;
[0034] 2) Add ammonia water to the hydrated ruthenium trichloride solution to adjust the pH of the solution to 9, and react for 30 minutes to obtain a solution with black precipitates;
[0035] 3) Centrifuge the solution in step 2) with a centrifuge at a speed of 10,000r / min for 10 minutes; the precipitate obtained by centrifugation is washed twice with water, and then centrifuged to obtain a black precipitate;
[0036] 4) Heating the precipitate obtained in step 3) in nitrogen gas at a heating temperature of 200°C for 2 hours to obtain nano-scale ruthenium dioxide;
[0037] 5) Take 0.01 g of the ruthenium dioxide obtained in step 4), and add 0.01 g of ovalbumin into 10 mL of water and sonicate for 30 minutes to obtain a ruthenium dioxide comp...
Embodiment 3
[0039] Preparation of ruthenium dioxide composite ovalbumin nanomaterials:
[0040] 1) Weigh 0.4g ruthenium trichloride hydrate, add 10mL distilled water, stir to dissolve completely, and obtain ruthenium trichloride hydrate solution;
[0041] 2) Add ammonia water to the hydrated ruthenium trichloride solution to adjust the pH of the solution to 9, and react for 30 minutes to obtain a solution with black precipitates;
[0042] 3) Centrifuge the solution in step 2) with a centrifuge at a speed of 10,000r / min for 10 minutes; the precipitate obtained by centrifugation is washed twice with water, and then centrifuged to obtain a black precipitate;
[0043] 4) Heating the precipitate obtained in step 3) in nitrogen gas at a heating temperature of 200°C for 2 hours to obtain nano-scale ruthenium dioxide;
[0044] 5) Take 0.05 g of the ruthenium dioxide obtained in step 4), and add 0.05 g of ovalbumin into 50 mL of water and sonicate for 30 minutes to obtain a ruthenium dioxide comp...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com