A technology of crystalline graphite and coarse concentrate, which is applied in chemical instruments and methods, solid separation, wet separation, etc., can solve the problems of difficulty in extracting fine flake graphite and excessive grinding of large flakes, so as to improve stability and reliability regulatory effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0044]Samples 1-3 were crushed and ground, and the upper limit of the grinding product’s particle size was 1 mm. Three groups of coarse concentrates were obtained under the same process conditions. The same process conditions were: one-stage roughing, during the roughing process, adding Water glass 2000g / t, kerosene 150g / t, No. 2 oil 75g / t; rougher concentrate and rougher tailings are obtained by roughing, and rougher concentrate is rough concentrate, and the rough concentrate is separated by gravity+ Flotation carries out "fine quality separation" operation, and "fine quality separation" operation adopts spiral quality separator. The quality separation process is as follows Figure 5 As shown, the results of fine quality classification are shown in Table 2.
[0045] Table 2 Raw ore fractionation test results under different fixed carbon content
[0046]
[0047] See Table 3 for the 0.15mm sieving results of the quality-separated products.
[0048] Table 3 0.15mm sieving ...
Embodiment 2
[0063] Taking sample 2 as an example, a full-process closed-circuit test was carried out, such as Figure 6 As shown, it specifically includes the following steps:
[0064] (1) One-stage roughing, during the roughing process, add water glass 2000g / t, kerosene 150g / t, No. 2 oil 75g / t; roughing to obtain roughing concentrate and roughing tailings, the roughing concentrate is Coarse concentrate, and use gravity separation + flotation to carry out "fine quality separation" operation on the coarse concentrate to obtain K coarse and K fine. The rough separation tailings are subjected to a stage of scavenging, and 1800g / t of water glass is added during the scavenging process. Kerosene 70g / t, No. 2 oil 40g / t, the final tailings and scavenging concentrate are obtained, and the scavenging concentrate is returned to roughing.
[0065] (2) K rough is re-grinded and re-selected after four stages: the grinding medium ratio is M 3~5mm :M 1~2mm =2:1, ball material ratio is M 球 :M 料 =4:1,...