Ceramic slurry having high firing finished product rate and used for grouting and preparation method thereof

A technology for finished products and mud, which is applied in the field of ceramic mud for grouting with high firing yield and its preparation field, can solve the problems of uneven structure distribution, low firing power, complex product shape, etc., and achieves guaranteed carbonization. Silicon particle size, high melting point, and the effect of reducing the amount of quartz

Active Publication Date: 2020-05-29
唐山市丰华陶瓷有限公司
View PDF5 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] However, the problem of low firing efficiency often occurs in the actual production process of products with complex shapes. This is due to the complex shape of the product, the different dehydration rates of different parts after the slurry is injected into the mold, and the solid particles in the slurry are superimposed and attached to the wall of the green body. The different layers make the internal structure distribution of the green body uneven. During the firing process, when the stress caused by the internal expansion and contraction of some products is concentrated on the section of the hierarchical structure, the structural section of the green body becomes larger, causing cracks or even direct cracking.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Ceramic slurry having high firing finished product rate and used for grouting and preparation method thereof
  • Ceramic slurry having high firing finished product rate and used for grouting and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0048] A method for preparing ceramic slurry for grouting with a high firing rate, comprising the following steps,

[0049] S1: 5 parts of quartz, 5 parts of waste porcelain powder, 5 parts of kaolin, 32 parts of ball clay, 30 parts of calcined coke gemstones, and 28 parts of water are mixed and ball-milled to obtain rough grinding mud;

[0050] S2: keep stirring the coarse grinding mud, and carry out aging. The aging time is 3 days. During the aging period, the coarse grinding mud is replenished with water according to the water evaporation of the coarse grinding mud, so as to keep the volume of the mud stable;

[0051] S3: Before grouting, add 20 parts of alumina mixed with chromium oxide powder, stir for 3 hours, add 0.02 parts of sodium polyacrylate, continue stirring for 1 hour, then add 6 parts of silicon carbide, and stir for 1 hour to obtain ceramic slurry for grouting.

[0052] Here, quartz, waste porcelain powder, kaolin, ball clay, and calcined coke are all powder m...

Embodiment 6

[0087] A preparation method of ceramic slurry for grouting with a high firing rate, based on Example 1, comprising the following steps, S1: 5 parts of quartz, 5 parts of waste porcelain powder, 5 parts of kaolin, and 32 parts of ball clay , 30 parts of calcined coke gemstones, 28 parts of water raw materials are mixed and ball milled to obtain rough grinding mud;

[0088] S2: keep stirring the coarse grinding mud, and carry out aging. The aging time is 3 days. During the aging period, the coarse grinding mud is replenished with water according to the water evaporation of the coarse grinding mud, so as to keep the volume of the mud stable;

[0089] S3: Before grouting, add 20 parts of alumina mixed with chromium oxide powder, stir for 4 hours, then add 6 parts of silicon carbide, stir for 1 hour, and obtain ceramic slurry for grouting.

Embodiment 7

[0091] A preparation method of ceramic slurry for grouting with a high firing rate, based on Example 1, comprising the following steps, S1: 5 parts of quartz, 5 parts of waste porcelain powder, 5 parts of kaolin, and 32 parts of ball clay , 30 parts of calcined coke gemstones, 28 parts of water raw materials are mixed and ball milled to obtain rough grinding mud;

[0092] S2: keep stirring the coarse grinding mud, and carry out aging. The aging time is 3 days. During the aging period, the coarse grinding mud is replenished with water according to the water evaporation of the coarse grinding mud, so as to keep the volume of the mud stable;

[0093] S3: Before grouting, add 20 parts of alumina mixed with chromium oxide powder, 0.02 part of sodium polyacrylate, and 6 parts of silicon carbide, and stir for 5 hours to obtain ceramic slurry for grouting.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Particle sizeaaaaaaaaaa
Granularityaaaaaaaaaa
Login to View More

Abstract

The invention relates to the technical field of grouting ceramics, and discloses ceramic slurry having high firing finished product rate and used for grouting. The problems that after existing slurryis poured into a complex mold, dehydration rates of different parts are different, the structure distribution in a blank body is not uniform, and cracks and even direct cracking are easily generated in the firing process are solved; the ceramic slurry is prepared by mixing the following raw materials in parts by mass: 5-8 parts of quartz, 5-8 parts of waste porcelain powder, 5-8 parts of kaolin, 32-35 parts of ball clay, 30-35 parts of calcined flint clay, 6-8 parts of silicon carbide, 20-30 parts of aluminum oxide and chromium oxide mixed powder and 35-42 parts of water, wherein the molar ratio of aluminum oxide to chromium oxide in the aluminum oxide and chromium oxide mixed powder is 0.9-1.1; when a green body obtained by slurry grouting is sintered, the aluminum oxide and chromium oxide mixed powder is firstly molten to form intermiscible eutectic which flows in gaps of the green body under the action of stress, so that the phenomenon of stress concentration is weakened, and the firing success rate of a finished product is increased. The invention further discloses a preparation method of the slurry, and the firing success rate of the finished product is increased.

Description

technical field [0001] The invention relates to the technical field of grouting ceramics, in particular to a high-firing ceramic slurry for grouting and a preparation method thereof. Background technique [0002] At present, the grouting method is also called the ceramic grouting molding method. The grouting method is a molding method in which the slurry is poured into a plaster mold to make it into a product. Therefore, the water in the part of the mud near the inner wall of the model is sucked by the porous gypsum to form a mud layer with the same shape as the inner wall of the model on the inner wall of the Shifen mold. This mud layer thickens with time. After stopping for a period of time, dump the excess mud, and the mud layer close to the inner wall of the Shifen model remains in the model; after a period of time, the mud layer naturally shrinks and separates from the model, and the formed rough billet take out. The grouting method is mainly suitable for batch moldin...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C04B33/132C04B33/13C04B33/28
CPCC04B33/1324C04B33/13C04B33/1305C04B35/63424C04B35/626C04B35/62807C04B35/62886C04B35/62675C04B33/28C04B2235/3418C04B2235/3217C04B2235/3241C04B2235/3826C04B2235/5436Y02P40/60
Inventor 王宝成
Owner 唐山市丰华陶瓷有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products