The technology of suspension stabilizer and concentrated liquid is applied in the field of suspension stabilizer of concrete waste slurry concentrate and its preparation, which can solve the problems of poor stability of concrete waste slurry concentrate, prone to moisture stratification, poor homogeneity, etc. Suspension and dispersion effect, reduction of bleeding stratification and compaction, and hydration inhibition effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] A preparation method of concrete waste slurry concentrate suspension stabilizer, the specific steps are as follows:
[0041] (1) Weigh 100g of glycerol and 2.8g of deionized water in the reaction vessel, stir and mix evenly, then add 12.6g of maltose and 1.4g of hydroxypropyl methylcellulose to it, heat up to 70°C, and continue to stir for 2h, to obtain a clear solution;
[0042] (2) Weigh 1.4g of chlorite and add it to the solution in step 1), and the rotating speed is 6000rpm and continues high-speed stirring for 1h to obtain a uniform suspension;
[0043] (3) Add 0.7g phosphorous acid to the suspension in step 2), stir for 5min, then continuously add 21g pyrophosphoric acid within 1h, control the reaction temperature at 70°C, and react for 8h to obtain a suspension of concrete waste slurry concentrate stabilizer.
Embodiment 2
[0045] A preparation method of concrete waste slurry concentrate suspension stabilizer, the specific steps are as follows:
[0046] (1) Weigh 100g of glycerol and 3.1g of deionized water in the reaction vessel, stir and mix evenly, then add 23.1g of lactose and 1.5g of hydroxypropyl cellulose to it, heat up to 80°C, and continue to stir for 4h to obtain a clear solution;
[0047] (2) take by weighing 1.5g illite and add it to the solution in step 1), and the rotating speed is 10000rpm and continues high-speed stirring for 3h to obtain a uniform suspension;
[0048] (3) Add 1.5g phosphoric acid to the suspension in step 2), stir for 10min, then continuously add 23.1g phosphorus trichloride within 2h, control the reaction temperature at 90°C, and react for 7h to obtain a concentrated concrete waste slurry Liquid suspension stabilizer.
Embodiment 3
[0050] A preparation method of concrete waste slurry concentrate suspension stabilizer, the specific steps are as follows:
[0051] (1) Weigh 100g of glycerol and 4.6g of deionized water in the reaction vessel, stir and mix evenly, then add 7.7g of sucrose and 4.6g of hydroxyethyl cellulose to it, heat up to 70°C, and continue to stir for 3h to obtain a clear solution;
[0052] (2) take by weighing 3.1g kaolinite and add it to the solution in step 1), and the rotating speed is 9000rpm and continues high-speed stirring for 2h to obtain a uniform suspension;
[0053] (3) 1.5g of sulfurous acid was added to the suspension in step 2), stirred for 8min, then 32.3g of phosphorus pentoxide was continuously added in 2h, the reaction temperature was controlled at 75°C, and the reaction was performed for 6h to obtain concrete waste slurry Concentrate suspension stabilizer.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com