A color-changing and flooring technology, which is applied in the field of home decoration materials, can solve the problems of poor artistic appreciation, short service life, and poor uniformity, and achieve the effects of improving three-dimensionality, easy operation, and simple manufacturing process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0045] A preparation method of a liquid floor variable color-changing decorative liquid, comprising the following steps:
[0046] 1) Add 1 part by weight of phthalocyanine green to the reaction kettle, then add 40 parts by weight of corn oil and 12 parts by weight of epoxy modified silicone resin, heat up to 60°C, adjust the rotation speed to 1200rpm, stir for 2 hours, and cool to room temperature. , the density is 1.155g / ml, and the viscosity is 8714CPS (25℃), that is, the green solution A is obtained;
[0047] 2) Add 2 parts by weight of anthocyanin to the reactor, add 40 parts by weight of deionized water, 8 parts by weight of short oil alkyd resin, 10 parts by weight of ethanol, adjust the pH to be 4.2, adjust the rotating speed to 500 rpm, and stir for 1 hour. , the density is 1.023g / ml, the viscosity is 213CPS (25℃), and it is the red solution B;
[0048] 3) Add 1 part by weight of heat-sensitive orange dye to the reaction kettle, add 30 parts by weight of gasoline, adj...
Embodiment 2
[0051] A preparation method of a liquid floor variable color-changing decorative liquid, comprising the following steps:
[0052] 1) Add 2 parts by weight of phthalocyanine green to the reaction kettle, then add 60 parts by weight of corn oil and 15 parts by weight of epoxy modified silicone resin, heat up to 80°C, adjust the rotation speed to 1500rpm, stir for 3 hours, and cool to room temperature. , the density is 1.165g / ml and the viscosity is 10134CPS (25℃), that is, the green solution A is obtained;
[0053] 2) Add 5 parts by weight of anthocyanin to the reactor, add 60 parts by weight of deionized water, 12 parts by weight of short oil alkyd resin, 15 parts by weight of ethanol, adjust the pH to be 4.4, adjust the rotating speed to be 800 rpm, stir for 1.5 hours, Detect that its density is 1.037g / ml, and its viscosity is 431CPS (25℃), that is, the red solution B is obtained;
[0054] 3) Add 1.5 parts by weight of heat-sensitive orange dye to the reaction kettle, add 40 ...
Embodiment 3
[0057] A preparation method of a liquid floor variable color-changing decorative liquid, comprising the following steps:
[0058] 1) Add 3 parts by weight of phthalocyanine green to the reaction kettle, then add 80 parts by weight of corn oil, 20 parts by weight of epoxy modified silicone resin, heat up to 120°C, adjust the rotation speed to 2000rpm, stir for 4 hours, and cool to room temperature. , the density is 1.207g / ml and the viscosity is 12671CPS (25℃), that is, the green solution A is obtained;
[0059] 2) Add 8 parts by weight of anthocyanin to the reaction kettle, add 80 parts by weight of deionized water, 15 parts by weight of short oil alkyd resin, 20 parts by weight of ethanol, adjust the pH to 4.6, adjust the rotating speed to 1200 rpm, and stir for 2 hours. , the density is 1.074g / ml, the viscosity is 728CPS (25℃), and the red solution B is obtained;
[0060] 3) Add 2 parts by weight of heat-sensitive orange dye to the reaction kettle, add 50 parts by weight of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com