Plant polyphenol-protein composite leather filler and preparation process thereof
A technology of plant polyphenols and fillers, applied in small raw hides/large raw hides/leather/fur treatment, small raw hides/large raw hides/leather hides/fur chemical treatment, tanning treatment, etc., can solve the problem of poor skin fiber binding force , The physical and mechanical properties of the finished leather are deteriorated, environmental pollution and other problems, and the finished leather is soft and plump, light in color, and good in physical and mechanical properties.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Add 300 parts of water into the reaction kettle with agitator and condenser, and adjust the pH value of the bath solution to 9.8 with an appropriate amount of sodium hydroxide aqueous solution; then add 100 parts of commercially available hydrolyzed protein into the reaction kettle to make it After fully dissolving, add 50 parts of bayberry extract, stir and mix evenly; control the reaction temperature at 18°C, and react for 1.5 hours to obtain a liquid product of plant polyphenol-protein composite leather filler, and then spray dry to obtain a solid powder product . The product has a pH value of 9.2, a hydrolyzed protein content of 59% by weight, and a tannin content of 21% by weight.
Embodiment 2
[0025] Add 300 parts of water into the reaction kettle with agitator and condenser, and adjust the pH value of the bath solution to 10.4 with an appropriate amount of sodium hydroxide aqueous solution; then add 100 parts of hydrolyzed protein extracted from raw hides into the reaction kettle , after fully dissolving it, add 55 parts of thick bark extract, stir and mix evenly; control the reaction temperature at 22°C, and react for 1.0 hour to obtain a liquid product of plant polyphenol-protein composite leather filler, which is then spray-dried Obtain solid powder product. The product has a pH value of 8.1, a hydrolyzed protein content of 55% by weight, and a tannin content of 26% by weight.
Embodiment 3
[0027] Add 300 parts of water into the reaction kettle with agitator and condenser, and adjust the pH value of the bath solution to 10.8 with an appropriate amount of potassium hydroxide aqueous solution; then add 100 parts of protein-containing waste from the tanning industry Add the extracted hydrolyzed protein into the reaction kettle to fully dissolve it, then add 70 parts of larch extract, stir and mix evenly; control the reaction temperature at 25°C, and react for 50 minutes to obtain the plant polyphenol-protein composite leather filling A liquid product, and then spray-dried to obtain a solid powder product. The product has a pH value of 10.0, a hydrolyzed protein content of 50% by weight, and a tannin content of 40% by weight.
PUM
Login to View More Abstract
Description
Claims
Application Information