Composite leather greasing agent and its prepn process
A technology of leather fatliquor and reagent, which is applied in the field of new compound leather fatliquor, can solve the problems of unsatisfactory thermodynamic stability of fatliquor, and achieve the effects of good filling performance, good adsorption capacity and stable quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Embodiment 1: the fatliquoring agent that sheepskin garment leather is used
[0025] Component Proportion ratio (parts by weight)
[0026] Polyoxyethylene alkyl phosphate 80
[0027] Cottonseed Oleamide 120
[0028] 52 # Chlorinated paraffin 150
[0029] Sodium cetyl sulfonate 40
[0030] Octylphenol polyoxyethylene ether (TX-10) 60
[0031] Olive Oil PEG 550
[0032] The preparation method is to mix polyoxyethylene alkyl phosphate and cottonseed oil amide evenly at 40±5°C, then add the mixed chlorinated paraffin and olive oil polyethylene glycol ester oil, and heat up to 50±5°C. ℃, mix evenly, then add TX-10 and sodium alkylsulfonate, mix and stir evenly at 40±5℃.
[0033] The polyoxyethylene alkyl phosphate is prepared according to the following method: in a synthesis kettle, quantitatively add fatty alcohol polyoxyethylene ether, and then heat it to 40°C until it melts evenly. Slowly add phosphorylation reagent phosphorus p...
Embodiment 2
[0037] Embodiment 2: Fatliquor for pigskin garment leather
[0038] Component Proportion ratio (parts by weight)
[0039] Polyoxyethylene alkyl phosphate 60
[0040] Cottonseed Oleamide 180
[0041] 52 #Chlorinated paraffin 90
[0042] Sodium dodecyl sulfonate 100
[0043] TX-10 50
[0044] Olive Oil PEG 70
[0045] 30 # Oil 400
[0046] The preparation method of the leather fatliquoring agent is to mix polyoxyethylene alkyl phosphate and cottonseed oil amide evenly at 40±5°C, and then add the mixed chlorinated paraffin and olive oil polyethylene glycol ester oil and 30 # Engine oil, heat up to 50±5°C, mix evenly, then add TX-10 and sodium alkylsulfonate, mix and stir evenly at 40±5°C.
[0047] The preparation of polyoxyethylene alkyl phosphate, cottonseed oil amide and olive oil polyethylene glycol ester is the same as in Example 1.
Embodiment 3
[0048] Embodiment 3: Fatliquor for cowhide sofa leather
[0049] Component Proportion ratio (parts by weight)
[0050] Polyoxyethylene alkyl phosphate 40
[0051] Cottonseed Oleamide 140
[0052] 52 # Chlorinated paraffin 40
[0053] Sodium dodecyl sulfonate 40
[0054] TX-10 80
[0055] The preparation method of leather fatliquoring agent is to mix polyoxyethylene alkyl phosphate and cottonseed oil amide at 40±5°C, then add chlorinated paraffin, heat up to 50±5°C, mix evenly, and then add TX -10 and sodium alkylsulfonate were mixed and stirred evenly at 40±5°C.
[0056] The polyoxyethylene alkyl phosphate is prepared according to the following method: in a synthesis kettle, quantitatively add fatty alcohol polyoxyethylene ether, and then heat it to 40°C until it melts evenly. Slowly add the phosphorylating reagent phosphorus oxychloride, the molar ratio of phosphorus oxychloride to fatty alcohol polyoxyethylene ether is 3:50, stir as it ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com