Single component silane modified polyether seal glue and its preparation method
A technology of silane-modified polyether and silane-terminated polyether, which is applied in the field of one-component silane-modified polyether sealant and its preparation, can solve the problem of pungent smell of polyurethane sealant and easy pollution of adjacent silicone sealant Parts, poor surface finish, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] Prepare a one-component silane-modified polyether sealant, which contains MS-polymer resin (KANEKA S303H), plasticizer (dioctyl phthalate), calcium carbonate, titanium dioxide, fumed silica, modified Organotin curing agent etc., the parts by weight ratio of described composition is as follows:
[0036] MS-polymer 38.5 parts
[0037] Dioctyl phthalate 13.3 parts
[0038] Calcium carbonate 40.2 parts
[0039] Titanium dioxide 4.1 parts
[0040] 0.5 parts of polyamide thixotropic agent
[0041] UV absorber 0.15 parts
[0042] UV stabilizer 0.15 parts
[0043] Fumed silica 2.2 parts
[0044] Vinyltrimethoxysilane 0.3 parts
[0045] N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane 0.5 parts
[0046] Modified organotin 0.1 parts
[0047] During preparation, sequentially add MS-polymer, dioctyl phthalate, titanium dioxide, ultraviolet absorber and stabilizer to a biaxial planetary stirring tank at room temperature, blend for 10-15 minutes under vacuum protection, and th...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com