Mosquito preventing fiber dyed yarn and its production process
A production method and yarn spinning technology, which is applied in the field of special functional melange spinning yarn and its production, can solve the problems of monotonous color, fabric color piece dyeing is not as rich and colorful as color spinning, and the mosquito repellent effect is weakened, etc., to achieve The effect of maintaining hygiene level, reducing biting, and good spinnability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
example 1
[0046] Example 1 (original white, bleached)
[0047] Select 120 kilograms of cotton loose fibers for use, put them into a solution with a bath ratio of 1:10 at normal temperature, add 2% penetrating agent JFC, 1% scouring agent SA, and adjust pH 10 to 11 with soda ash or caustic soda (for bleaching, add hydrogen peroxide 10g / L), keep warm at 98°C for 30 minutes, let off the corner water, wash with water, neutralize with acetic acid and wash with water until neutral. After treatment, add low-temperature fixative HS-AM 30g / L to fully dilute, stir and keep warm for 5-6 minutes, then add penetrant JINTEX AM 30g / L and keep warm for 5-6 minutes, finally add 40g / LCAT-AM, and let it go after 10 minutes Corner water, dehydration, requires a moisture content of 40% to 60%, spray 0.5% antistatic agent TF-480A and 0.5% hydrophilic soft oil FK-2880 into the dehydrator, and dry at a temperature higher than 120°C faster.
example 2
[0048] Example 2 (whitening or dyeing)
[0049] Choose 140 kilograms of cotton sliver loose fibers for use, put it into a solution with a bath ratio of 1:8 and 2 g / liter of chelating dispersant CT powder (soft water effect) at room temperature, add penetrating agent JFC 2%, scouring agent SA 1% Use soda ash or caustic soda to adjust the pH to 10-11 (add hydrogen peroxide 10g / L at 60°C for bleaching), keep warm at 98°C for 30 minutes, let off the corner water, and use the conventional cotton loose fiber dyeing process, add low-temperature fixative HS-AM for post-treatment 30g / L is fully diluted, stirred and kept warm for 5-6 minutes, then added penetrant JINTEX AM30g / L and kept warm for 5-6 minutes, and finally added 40g / L CAT-AM, let off the corner water after 10 minutes, and dehydrated. 40% to 60%, spray 0.5% antistatic agent TF-480A and 0.5% hydrophilic soft oil FK-2880 into the dehydrator, and the drying requires a higher temperature of 120°C and a faster speed.
[0050] T...
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com