A wood lacquer and model technology, applied in the field of wood lacquer, can solve the problems of insufficient safety and environmental protection, poor antibacterial effect, poor stain resistance of the paint film, etc., and achieve the effect of perfect decoration, unique formula and smooth paint film
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Equipped with 100kg wood lacquer of the present invention, it is formulated by the raw material of following weight content:
[0027] Modified saturated polyester resin 72.6kg, mixture of n-butyl acetate and propylene glycol methyl ether acetate 16kg, modified polyurethane dispersant 0.5kg, polyamide wax anti-settling agent 0.6kg, fumed silica matting powder 5kg, polytetrafluoroethylene Vinyl fluoride wax powder 1kg, bubble breaking polysiloxane solution 0.2kg, polyether modified polydiylsiloxane and polyester modified polydiylsiloxane mixed solution 0.3kg, nano silver antibacterial agent 0.3kg, more Functional anion additive 0.5kg, vinyl acetate resin 3kg.
[0028] Feed according to the order of the conventional paint making process, each material is stirred evenly, and then another material is added, and the material is stirred while feeding, and the viscosity is detected after the dispersion is uniform to obtain the wood varnish of the present invention.
Embodiment 2
[0030] Equipped with 100kg wood lacquer of the present invention, it is formulated by the raw material of following weight content:
[0031] Modified saturated polyester resin 77.0kg, mixture of n-butyl acetate and propylene glycol methyl ether acetate 10kg, modified polyurethane dispersant 1.0kg, polyamide wax anti-settling agent 1.0kg, fumed silica matting powder 6kg, polytetrafluoroethylene Vinyl fluoride wax powder 1kg, bubble breaking polysiloxane solution 0.4kg, polyether modified polydiylsiloxane and polyester modified polydiylsiloxane mixed solution 0.4kg, nano silver antibacterial agent 0.4kg, more 0.8kg of functional anion additives, 2kg of vinyl acetate resin.
[0032] Feed according to the order of the conventional paint making process, each material is stirred evenly, and then another material is added, and the material is stirred while feeding, and the viscosity is detected after the dispersion is uniform to obtain the wood varnish of the present invention.
Embodiment 3
[0034] Equipped with 100kg wood lacquer of the present invention, it is formulated by the raw material of following weight content:
[0035] Modified saturated polyester resin 71.4kg, mixture of n-butyl acetate and propylene glycol methyl ether acetate 10kg, modified polyurethane dispersant 1.0kg, polyamide wax anti-settling agent 1.2kg, fumed silica matting powder 8kg, polytetrafluoroethylene Vinyl fluoride wax powder 1.5kg, foam breaking polysiloxane solution 0.4kg, polyether modified polydiylsiloxane and polyester modified polydiylsiloxane mixed solution 0.5kg, nano silver antibacterial agent 0.5kg, 1.5kg of multifunctional anion additives, 4kg of vinyl acetate resin.
[0036] Feed according to the order of the conventional paint making process, each material is stirred evenly, and then another material is added, and the material is stirred while feeding, and the viscosity is detected after the dispersion is uniform to obtain the wood varnish of the present invention.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com