An asphalt rejuvenator, common technology, applied in building components, building insulation materials, buildings, etc., can solve environmental hazards, high-quality asphalt waste and other problems, and achieve the effects of preventing pollution, restoring the service life of road surfaces, and protecting forest land
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] A common asphalt rejuvenator of this embodiment, which is mainly prepared by heating, mixing and stirring the following components in parts by mass:
[0023] Esso 70# new asphalt 30 copies
[0024] 65 parts of recycled oil
[0025] 4 parts dibutyl phthalate and
[0026] 1 part of high temperature stabilizer.
[0027] The above-mentioned regenerated oil is a vacuum oil obtained by fractionating crude oil through a vacuum device, wherein the aromatic content is 44.76%, and the high flash point is above 220° C.; the above-mentioned high-temperature stabilizer is sasobit. Sasobit is a new type of polyolefin high temperature stabilizer, its chemical composition is synthetic long-chain saturated hydrocarbons, and its dropping melting point is 115°C.
[0028] The preparation method of the common asphalt rejuvenator of the above-mentioned present embodiment comprises the following steps: firstly, heating 30 parts of Esso 70# fresh asphalt at 115° C. for 3 hours, and stirring...
Embodiment 2
[0030] A common asphalt rejuvenator of this embodiment, the common asphalt rejuvenator is mainly prepared by mixing, heating and stirring the following components in parts by mass:
[0031] Esso 70# new asphalt 23 parts
[0032] Regenerated oil 72 parts
[0033] 3 parts dibutyl phthalate and
[0034] High temperature stabilizer 2 parts.
[0035] The above regenerated oil is a vacuum oil obtained by fractionating crude oil through a vacuum device, wherein the aromatic content is 44.76%, and the high flash point is above 220°C; the above high temperature stabilizer is Sasobit.
[0036] The preparation method of the common asphalt rejuvenator of the above-mentioned present embodiment comprises the following steps: firstly, heating 23 parts of Esso 70# fresh asphalt at 135° C. for 2 hours, and stirring evenly; then, mixing 72 parts of regenerated oil, Heat 3 parts of dibutyl phthalate and 2 parts of high-temperature stabilizer at 135°C for 1 hour, and stir evenly to obtain a mi...
Embodiment 3
[0038] A common asphalt rejuvenator of this embodiment, the common asphalt rejuvenator is mainly prepared by mixing, heating and stirring the following components in parts by mass:
[0039] Esso 70# new asphalt 35 copies
[0040] 60 parts of recycled oil
[0041] 3 parts dibutyl phthalate and
[0042] High temperature stabilizer 2 parts.
[0043]The above regenerated oil is a vacuum oil obtained by fractionating crude oil through a vacuum device, wherein the aromatic content is 44.76%, and the high flash point is above 220°C; the above high temperature stabilizer is Sasobit.
[0044] Except for the difference in the ratio of all raw materials, the preparation method of this example is exactly the same as that of Example 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com