Method for preparing water-based UV (Ultraviolet) pigment printing paste for textile use
A paint printing, water-based technology, applied in the field of textile printing and dyeing, can solve the problems of high viscosity of UV color paste, incomplete curing, poor fabric feel, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Mix 15 parts of urethane acrylate, 2 parts of sodium alkylbenzene sulfonate, and 83 parts of deionized water, stir at 800r / min for 10 minutes, and then ultrasonicate the mixture for 20 minutes with an ultrasonic power of 800W to obtain a water-based urethane acrylate emulsion .
[0021] Pre-disperse 15 parts of Pigment Red 122, 12 parts of sodium dodecylsulfonate and 73 parts of deionized water at room temperature using a homogenizer at a speed of 6000r / min for 10 minutes, and transfer them to a circulating sand mill , grind for 2 hours, and the speed of the sand mill is 2400r / min to obtain the water-based pigment red paste.
[0022] Add 15 parts of water-based pigment red paste, 5 parts of water-based initiator 819DW, and 10 parts of thickener PBD to 70 parts of polyurethane acrylate emulsion, and stir for 15 minutes at a speed of 1000r / min to obtain water-based UV printing color pulp.
[0023] Transfer the water-based UV pigment printing paste to the fabric through ...
Embodiment 2
[0025] Mix 20 parts of urethane acrylate, 3 parts of sodium alkylbenzene sulfonate, and 77 parts of deionized water, stir at 1000r / min for 10 minutes, and then ultrasonicate the mixture for 20 minutes with an ultrasonic power of 800W to obtain a water-based urethane acrylate emulsion .
[0026] Weigh 13 parts of Pigment Yellow 83, 11 parts of sodium dodecylsulfonate and 76 parts of deionized water, pre-disperse at room temperature with a homogenizer at a speed of 6000r / min for 10min, and transfer to a circulating sand mill In the machine, grind for 3 hours, the speed of the sand mill is 2400r / min, and the water-based pigment yellow paste is obtained.
[0027] Add 15 parts of water-based pigment yellow paste, 3 parts of water-based initiator 2529, 2 parts of initiator 819DW, and 10 parts of thickener PBD to 70 parts of polyurethane acrylate emulsion, and stir for 15 minutes at a speed of 1000r / min. A water-based UV printing paste is prepared.
[0028] Transfer the water-based...
Embodiment 3
[0030] Mix 15 parts of polyurethane acrylate, 3 parts of sodium alkylbenzene sulfonate, 2 parts of sorbitan fatty acid ester, and 80 parts of deionized water, stir at 2000r / min for 10min, then ultrasonicate the mixture for 15min, and ultrasonically The power is 1000W to obtain water-based polyurethane acrylate emulsion.
[0031] Pre-disperse 19 parts of Pigment Blue 15:4, 11 parts of dispersant NNO and 70 parts of deionized water at room temperature using a high-speed homogenizer at a speed of 3000r / min for 10 minutes, and transfer to a circulating sand mill , grind for 3 hours, and the speed of the sand mill is 2400r / min, to obtain the blue slurry of water-based pigment.
[0032] Add the above-mentioned 13 parts of water-based pigment blue paste, 5 parts of water-based initiator 819DW, and 10 parts of thickener PBD to 72 parts of polyurethane acrylate emulsion, and use a fast mixer to stir at 1000r / min for 15 minutes to prepare Obtain water-based UV pigment printing paste. ...
PUM
| Property | Measurement | Unit |
|---|---|---|
| color fastness | aaaaa | aaaaa |