A processing method of flame retardant and fireproof calcium silicate board
A technology of calcium silicate board and processing method, which is applied in the direction of chemical instruments and methods, floor coverings, adhesive types, etc., can solve the problems of formaldehyde exceeding the standard, difficult to control, unable to withstand blisters, difficult to relocate, etc., and achieve low production cost , prevent formaldehyde from exceeding the standard, and increase the effect of aesthetics
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0021] Please combine figure 1 Shown, a kind of processing method of flame retardant and fireproof calcium silicate board, comprises the following steps:
[0022] (1) Firstly, put the calcium silicate board and veneer into the hot press in the order that the first and third layer materials are rootstock skin, and the second layer material is calcium silicate board;
[0023] (2) Prepare the adhesive mixture, mix the unsaturated resin and cellulose cotton at a mass ratio of 10:1, inject it into the gap between the calcium silicate board and the veneer in the constant temperature hot press, and perform curing treatment for 12 minutes. The treatment temperature is 110 ℃, pressure 8KPa, to achieve the balance of cold and heat shrinkage of calcium silicate board;
[0024] (3) After using a hot press for pasting, cool down to 55°C at a rate of 1°C / min, and then release the mold to obtain a rough plate;
[0025] (4) Trimming the rough slabs with an orbital trimming machine, cutting ...
Embodiment 2
[0028] Please combine figure 1 Shown, a kind of processing method of flame retardant and fireproof calcium silicate board, comprises the following steps:
[0029] (1) Firstly, put the calcium silicate board and veneer into the hot press in the order that the first and third layer materials are rootstock skin, and the second layer material is calcium silicate board;
[0030] (2) Prepare the adhesive mixture, mix the unsaturated resin and cellulose cotton with a mass ratio of 10:7, inject it into the gap between the calcium silicate board and the veneer in the constant temperature hot press, and perform curing treatment for 25 minutes. The treatment temperature is 130 ℃, pressure 13KPa, to achieve the balance of cold and heat shrinkage of calcium silicate board;
[0031] (3) After glueing with a constant temperature hot press, cool down to 65°C at a speed of 2°C / min, and then release the mold to obtain a rough plate;
[0032] (4) Trimming the rough slabs with an orbital trimmi...
Embodiment 3
[0035] Please combine figure 1 shown, please combine figure 1 Shown, a kind of processing method of flame retardant and fireproof calcium silicate board, comprises the following steps:
[0036] (1) Firstly, put the calcium silicate board and veneer into the hot press in the order that the first and third layer materials are rootstock skin, and the second layer material is calcium silicate board;
[0037] (2) Prepare the adhesive mixture, mix the unsaturated resin and cellulose cotton at a mass ratio of 10:3, inject it into the gap between the calcium silicate board and the veneer in the constant temperature hot press, and perform curing treatment for 18 minutes. The treatment temperature is 120 ℃, pressure 10KPa, to achieve the balance of cold and heat shrinkage of calcium silicate board;
[0038] (3) After glueing with a constant temperature hot press, cool down to 60°C at a speed of 1.5°C / min, and then release the mold to obtain a rough plate;
[0039] (4) Trimming the ro...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 