Method for preventing rabbit hair fabrics from hair shedding

A technology for preventing hair loss and rabbit hair, applied in animal fibers, textiles and papermaking, fiber processing and other directions, it can solve problems such as the limitation of application scope, and achieve the effects of reducing mutual slippage, long-lasting function, and reducing hair loss rate.

Inactive Publication Date: 2014-05-14
SOUTHWEST UNIVERSITY
View PDF3 Cites 5 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Therefore, the scope of application of

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for preventing rabbit hair fabrics from hair shedding
  • Method for preventing rabbit hair fabrics from hair shedding

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0021] Example 1: A method for preventing shed hair from rabbit fur fabric, which is processed according to the following steps:

[0022] Rabbit fur surface pretreatment: soak the rabbit fur fabric to be treated in a sulfuric acid solution with a mass fraction of 2%, bath ratio 1:50, pretreatment at 60℃ for 5 min, rinse with distilled water to pH 7, and dry treatment at 60℃ 120min.

[0023] Rabbit hair graft modification: mix 2% sucrose fatty acid ester glycidyl ether of rabbit hair fabric, 2% milk protein, 2% O-9 flat and O, control pH value of 7, rabbit hair The bath ratio of the fabric to the mixed solution is 1:50. The rabbit fur fabric is water bathed at 60°C for 40 minutes; dried at 60°C for 120 minutes, and then baked and grafted at 100°C for 20 minutes. Wash the baked rabbit fur fabric three times with water, and then bake it at 60°C for 120 minutes.

Embodiment 2

[0024] Example 2: A method for preventing shed hair from rabbit fur fabric, which is processed according to the following steps:

[0025] Rabbit fur surface pretreatment: soak the rabbit fur fabric to be treated in 0.5% sulfuric acid solution, bath ratio 1:50, pretreatment at 60℃ for 2 min, rinse with distilled water to pH 8, and dry treatment at 60℃ 110min.

[0026] Rabbit hair graft modification: mix 0.5% sucrose fatty acid ester glycidyl ether of rabbit hair fabric, 0.5% sericin, 0.5% O-10 flat and O, control the pH value of 8, rabbit The bath ratio of the wool fabric to the mixed solution is 1:50. The rabbit wool fabric is dried in a water bath at 60°C for 35 minutes; dried at 60°C for 110 minutes, and then baked and grafted at a temperature of 90°C for 20 minutes. Wash the baked rabbit fur fabric 4 times with water, and then bake it at 60°C for 120 minutes.

Embodiment 3

[0027] Example 3: A method for preventing shed hair from rabbit fur fabric, which is processed according to the following steps:

[0028] Rabbit fur surface pretreatment: soak the rabbit fur fabric to be treated in 5% sulfuric acid solution, bath ratio 1:50, pretreatment at 60℃ for 2 min, rinse with distilled water to pH 6, and dry treatment at 60℃ 130min.

[0029] Rabbit hair grafting modification: mix 0.5% sucrose fatty acid ester glycidyl ether of rabbit hair fabric, 5% collagen, 5% O-20 type flat and O, control pH value of 6, rabbit hair The bath ratio of the fabric to the mixed solution is 1:50. The rabbit fur fabric is water bathed at 60°C for 35 minutes; dried at 60°C for 130 minutes, and then baked at 110°C for 20 minutes. Wash the baked rabbit fur fabric 5 times with distilled water, and then bake it at 60°C for 120 minutes.

[0030] From figure 1 with figure 2 It can be seen that before the treatment, the surface of the rabbit fur fabric was a smooth scaly layer; after t...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to a method for preventing rabbit hair fabrics from hair shedding, which comprises the following steps: soaking the rabbit hair fabric to be treated in a sulfuric acid solution, performing pretreatment of the rabbit hair surface, then performing water bath of the rabbit hair fabric with a cross-linking agent with a mass fraction of 0.5-5% of the rabbit hair fabric, protein with a mass fraction of 0.5-10%, and a surfactant with a mass fraction of 0.5-10% according to a bath ratio of 1:50 at a temperature of 60 DEG C for 30 min-50 min, drying, and performing roasting and grafting at 90-110 DEG C for 20 min. The method of the invention prolongs the duration of the anti-hair shedding function of rabbit hair fabrics, causes no damage to the rabbit hair fabrics, and can improve fiber strength. The method is simple and easy to operate.

Description

Technical field [0001] The invention relates to a method for preventing hair loss of a wool fabric, in particular to a method for preventing hair loss of a rabbit fur fabric, and belongs to the fabric finishing technology. Background technique [0002] With the continuous improvement of modern living standards and people’s cultural accomplishments, people’s pursuit of clothing products is developing in the direction of "light, soft, warm, cool, and beautiful". Rabbit fur products have all the advantages of these five aspects. The pursuit of ideal clothing fabrics. Rabbit hair is a high-grade textile material in my country. The rabbit hair fabric feels smooth, soft, light and fluffy, has a unique appearance, luxurious and generous, good warmth retention and moisture absorption, giving people a high-grade product enjoyment. Due to the smooth surface of the rabbit hair fiber, small friction coefficient, low number of crimps, poor cohesion, etc., the hair removal phenomenon of the r...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): D06M15/15D06M15/53D06M11/55D06M101/12
Inventor 张同华李佳丽李铭涵张光先
Owner SOUTHWEST UNIVERSITY
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products