Environmental-friendly dry-hanging adhesive and preparation method thereof
A dry-hanging adhesive and environmental-friendly technology, which is applied in the direction of epoxy resin glue, adhesive, adhesive type, etc., can solve the problems of short use time of dry-hanging glue, insufficient adhesion, easy cracking of the coating, etc., to achieve Low limit of harmful substances, strong adhesive force and long service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
specific Embodiment approach
[0026] An environment-friendly dry-hanging adhesive, which is made by mixing the main paint and curing agent in a mass ratio of 2:0.8-1.2, wherein the main paint and curing agent are prepared by the following components and weight ratios:
[0027] Wherein the main paint component and parts by weight ratio are as follows:
[0028]
[0029] Wherein curing agent component and parts by weight ratio are as follows:
[0030]
[0031]
[0032] The preparation method of above-mentioned environment-friendly type dry-hanging adhesive comprises the following steps:
[0033] (1), the main paint is prepared according to the following preparation method:
[0034] Add epoxy resin, epoxy reactive diluent, benzyl alcohol, anti-sedimentation agent, bentonite, quartz sand, heavy calcium, talcum powder, synthetic fiber, epoxy carbon black slurry into the container in sequence, and mix in the mixer at 1000- Disperse at 1200 rpm for 10-15 minutes until evenly mixed;
[0035] (2), curing...
Embodiment 1
[0040] Embodiment 1: An environment-friendly dry-hanging glue is formed by mixing the main paint and the curing agent in a mass ratio of 2:1, wherein the main paint and the curing agent are formulated by the following components and weight and number ratios:
[0041] Wherein the main paint component and parts by weight ratio are as follows:
[0042]
[0043]
[0044] Wherein curing agent component and parts by weight ratio are as follows:
[0045]
[0046] The preparation method of above-mentioned environment-friendly dry-hanging adhesive comprises the steps:
[0047] (1), the main paint is prepared according to the following preparation method:
[0048] 30 parts of epoxy resin, 4 parts of epoxy reactive diluent, 3 parts of benzyl alcohol, 1 part of anti-settling agent, 2.5 parts of bentonite, 10 parts of quartz sand, 50 parts of heavy calcium, 9.7 parts of talcum powder, 0.2 parts of synthetic fiber, Add 5 parts of epoxy carbon black slurry to the container in sequ...
Embodiment 2
[0055] Embodiment 2: An environment-friendly dry-hanging glue, which is formed by mixing the main paint and the curing agent in a mass ratio of 2:0.8, wherein the main paint and the curing agent are formulated by the following components and weight and number ratios:
[0056] Wherein the main paint component and parts by weight ratio are as follows:
[0057]
[0058] Wherein curing agent component and parts by weight ratio are as follows:
[0059]
[0060]
[0061] The preparation method of above-mentioned environment-friendly dry-hanging adhesive comprises the steps:
[0062] (1), the main paint is prepared according to the following preparation method:
[0063] 34 parts of epoxy resin, 3 parts of epoxy active diluent, 4 parts of benzyl alcohol, 1 part of anti-settling agent, 2.5 parts of bentonite, 10.7 parts of quartz sand, 30 parts of heavy calcium, 8 parts of talcum powder, 0.2 parts of synthetic fiber, Add 3 parts of epoxy carbon black slurry to the container in...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.