A manufacturing process and technology of kraft paper, applied in papermaking, papermaking machines, adding water repellents, etc., can solve the problems of unfavorable use, difficult to treat waste water, high cost of kraft paper, improve water resistance, reduce porosity, and improve water resistance. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] The manufacturing process of the water-resistant kraft paper comprises the following steps:
[0027] (1) Select raw materials: choose kraft bleached softwood pulp, hardwood pulp and bamboo pulp, the weight ratio of kraft bleached softwood pulp, hardwood pulp and bamboo pulp is 1: 1:0.3;
[0028] (2) Raw material mixing and beating: Put the kraft-bleached coniferous wood pulp, hardwood pulp and bamboo pulp into the pulping tank according to the ratio described in step (1), and add industrial water into the pulping tank, and stir Mix evenly to obtain a mixed slurry, and the concentration of the mixed slurry is 1.5%;
[0029] (21) The mixed slurry obtained in step (2) is first transported to the slurry storage tank, and the cationic emulsion rosin gum is put into the slurry storage tank, and stirred and mixed evenly, the concentration of the cationic emulsion rosin gum reaches 0.25%;
[0030] (22) Transporting the slurry obtained in step (21) to a fiber separator for coar...
Embodiment 2
[0034] The manufacturing process of the water-resistant kraft paper comprises the following steps:
[0035] (1) Select raw materials: choose kraft bleached softwood pulp, hardwood pulp and bamboo pulp, the weight ratio of kraft bleached softwood pulp, hardwood pulp and bamboo pulp is 1: 1:0.5;
[0036] (2) Raw material mixing and beating: Put the kraft-bleached coniferous wood pulp, hardwood pulp and bamboo pulp into the pulping tank according to the ratio described in step (1), and add industrial water into the pulping tank, and stir Mix evenly to obtain a mixed slurry, and the concentration of the mixed slurry is 2.2%;
[0037] (21) The mixed slurry obtained in step (2) is first transported to the slurry storage tank, and the cationic emulsion rosin gum is put into the slurry storage tank, and stirred and mixed evenly, the concentration of the cationic emulsion rosin gum reaches 0.3%;
[0038] (22) Transporting the slurry obtained in step (21) to a fiber separator for coars...
Embodiment 3
[0042] The manufacturing process of the water-resistant kraft paper comprises the following steps:
[0043] (1) Selection of raw materials: choose kraft bleached softwood pulp, hardwood pulp and bamboo pulp, the weight ratio of kraft bleached softwood pulp, hardwood pulp and bamboo pulp is 1: 1: 0.7;
[0044] (2) Raw material mixing and beating: put the kraft-bleached coniferous wood pulp, hardwood pulp and bamboo pulp into the pulping tank according to the ratio described in step (1), and add industrial water into the pulping tank, and stir Mix evenly to obtain a mixed slurry, and the concentration of the mixed slurry is 3.0%;
[0045] (21) The mixed slurry obtained in step (2) is first transported to the slurry storage tank, and the cationic emulsion rosin gum is put into the slurry storage tank, and stirred and mixed evenly, the concentration of the cationic emulsion rosin gum reaches 0.35%;
[0046](22) Transporting the slurry obtained in step (21) to a fiber separator fo...