Damp-proofing displacement-proofing corrugated carton
A technology for corrugated and corrugated cardboard, applied in the field of carton production, can solve the problems of low cardboard strength and slow drying speed, and achieve the effects of simple method, fast drying and high bonding strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Corrugated boxes, including corrugated paperboard, made of corrugated paper and containerboard bonded by an adhesive prepared from the following raw materials in parts by weight:
[0017] 45 parts of corn starch, 0.15 parts of borax, 0.08 parts of polydimethylsiloxane, 4.5 parts of sodium hypochlorite, 3 parts of potassium permanganate, 0.75 parts of quicklime, 2 parts of nano sepiolite powder, 0.2 parts of carboxymethyl cellulose, water 100 copies.
[0018] Preparation method: dissolve cornstarch in water and stir evenly; add sodium hypochlorite and potassium permanganate, heat to 30°C, stir for 15 minutes; keep at 30°C, add borax, stir for 16 minutes; add nano sepiolite powder, carboxymethyl cellulose , quicklime and polydimethylsiloxane, stirred for 5 minutes, and stood still for 10 hours to obtain corrugated cardboard adhesive.
Embodiment 2
[0020] Corrugated boxes, including corrugated paperboard, made of corrugated paper and containerboard bonded by an adhesive prepared from the following raw materials in parts by weight:
[0021] 35 parts of corn starch, 0.12 parts of borax, 0.05 parts of polydimethylsiloxane, 3 parts of sodium hypochlorite, 2 parts of potassium permanganate, 0.5 parts of quicklime, 1.5 parts of nano sepiolite powder, 0.1 part of carboxymethyl cellulose, water 100 copies.
[0022] Preparation method: Dissolve cornstarch in water, stir well; add sodium hypochlorite and potassium permanganate, heat to 30°C, stir for 20 minutes; keep at 35°C, add borax, stir for 16 minutes; add nano sepiolite powder, carboxymethyl cellulose , quicklime and polydimethylsiloxane, stirred for 5 minutes, and stood still for 10 hours to obtain corrugated cardboard adhesive.
Embodiment 3
[0024] Corrugated boxes, including corrugated paperboard, made of corrugated paper and containerboard bonded by an adhesive prepared from the following raw materials in parts by weight:
[0025] 55 parts of corn starch, 0.18 parts of borax, 0.1 part of polydimethylsiloxane, 6 parts of sodium hypochlorite, 4 parts of potassium permanganate, 1 part of quicklime, 2.5 parts of nano sepiolite powder, 0.3 parts of carboxymethyl cellulose, water 100 copies.
[0026] Dissolve cornstarch in water and stir evenly; add sodium hypochlorite and potassium permanganate, heat to 35°C, and stir for 10 minutes; keep at 30°C, add borax, and stir for 16 minutes; add nano sepiolite powder, carboxymethyl cellulose, quicklime and Polydimethylsiloxane, stirred for 5 minutes, and allowed to stand for 10 hours to obtain corrugated cardboard adhesive.
PUM

Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com