A mop, bamboo and hemp technology, applied in the field of fabrics, can solve the problems that water is not easy to evaporate, affect the beauty of home decoration, affect people's lives, etc., and achieve the effects of excellent water absorption, preventing the reproduction of bacteria and increasing comfort.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0036] The present invention also provides a kind of preparation method of mop cloth, comprises the following steps:
[0037] The bamboo, linen and cotton blended yarn is plyed into threads, and then knitted to obtain a mop cloth; the blended mass ratio of bamboo fiber, hemp fiber and cotton fiber in the bamboo, linen and cotton blended yarn is 10 to 70:10 to 60 : 20~40, the yarn count of described bamboo linen cotton blended yarn is 10 S ~40 S , the number of joint shares of the joint shares is 2 to 4 shares.
[0038]The present invention adopts bamboo hemp cotton blended yarn as the yarn in the mop cloth (abbreviated as mop yarn), wherein the blended mass ratio of bamboo fiber, hemp fiber and cotton fiber is 10~70:10~60:20~40, Preferably it is 20-60:10-40:20-40. In an embodiment of the present invention, the blended mass ratio of bamboo fiber, hemp fiber and cotton fiber in the bamboo hemp cotton blended yarn may be 40:20:40, 35:30:35 or 50:30:20. The yarn count of the m...
Embodiment 1
[0051] The ramie fiber is selected for degumming, and then the degummed lean hemp is cut and loosened to obtain the pretreated hemp fiber. Among them, the cutting length is 40 mm, and the number of opening channels is 6; the average length is controlled at 29-38 mm.
[0052] Based on 100% by weight, bamboo fibers, pretreated ramie fibers and cotton fibers are selected in a ratio of 40:20:40, and various fibers are evenly stacked in the plucking machine, and after grasping, mixing, opening, and impurity removal and carding to make slivers. Among them, in the blowing-carding process, the distance between the doffer and the cylinder is 4 mm, the speed ratio of the cylinder and the licker-in roller is 1:2, and the speed of the carding licker-in roller is 1000 rpm; the weight of the sliver produced is controlled 19g / 5m.
[0053] The cotton slivers made are made into mature slivers on the drawing frame, and the number of drawing lines is 3, and the output dry weight is 18 grams / 5 ...
Embodiment 2
[0073] The ramie fiber is selected for degumming, and then the degummed lean hemp is cut and loosened to obtain the pretreated hemp fiber. Among them, the cutting length is 45 mm, and the number of opening channels is 4; the average length is controlled at 29-40 mm.
[0074] Based on 100% by weight, bamboo fiber, pretreated ramie fiber and cotton fiber are selected in a ratio of 35:30:35, and all kinds of fibers are evenly stacked in the plucking machine, after grabbing, mixing, opening, and removing impurities and carding to make slivers. Among them, in the blowing-carding process, the distance between the doffer and the cylinder is 4 mm, and the speed of the carding roller is 950 rpm; the weight of the sliver produced is controlled at 21 grams / 5 meters.
[0075] The cotton slivers made are made into mature slivers on the drawing frame, the number of drawing lines is 2, and the output dry weight is 20 grams / 5 meters.
[0076] The prepared sliver is spun into a roving, the d...