Concrete water reducer and preparation method thereof
A concrete water-reducing agent and water-reducing agent technology, applied in the field of concrete additives, can solve the problems of poor plasticizing effect, single performance, difficult to control, etc. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] A concrete water reducer, which is made by mixing the following raw materials in parts by weight:
[0032] Polycarboxylate superplasticizer 40 parts
[0033] Sodium alkylbenzene sulfonate 10 parts
[0034] Sodium carboxymethyl cellulose 3 parts
[0035] Calcium formate 5 parts
[0036] Ethylene glycol 7 parts
[0037] 10 parts of triterpene saponins
[0038] Mass concentration is 20 parts of citric acid solution of 98%
[0039] Aluminum sulfate 5 parts
[0040] 3 parts cellulose ether
[0041] 50 parts of water.
[0042] Wherein, the weight average molecular weight of the polycarboxylate water reducer is 15,000-80,000.
[0043] A preparation method of concrete water reducer, comprising the following steps:
[0044] (1) Add polycarboxylate superplasticizer, sodium alkylbenzene sulfonate, sodium carboxymethyl cellulose, calcium formate, low molecular weight alcohol and aluminum sulfate in the reaction kettle in sequence, heat and stir to 30°C , keep stirring for...
Embodiment 2
[0048] A concrete water reducer, which is made by mixing the following raw materials in parts by weight:
[0049] Polycarboxylate superplasticizer 30 parts
[0050] Sodium alkylbenzene sulfonate 7 parts
[0051] Sodium carboxymethyl cellulose 5 parts
[0052] Calcium formate 1 part
[0053] Glycerol 15 parts
[0054] 3 parts triterpene saponins
[0055] Mass concentration is 10 parts of citric acid solution of 98%
[0056] 3 parts aluminum sulfate
[0057] xanthan gum 2 parts
[0058] 40 parts of water.
[0059] Wherein, the weight average molecular weight of the polycarboxylate water reducer is 15,000-80,000.
[0060] A preparation method of concrete water reducer, comprising the following steps:
[0061] (1) Add polycarboxylate superplasticizer, sodium alkylbenzene sulfonate, sodium carboxymethylcellulose, calcium formate, low molecular weight alcohol and aluminum sulfate in the reaction kettle in sequence, heat and stir to 40°C, Keep stirring for 30min;
[0062] ...
Embodiment 3
[0065] A concrete water reducer, which is made by mixing the following raw materials in parts by weight:
[0066] Polycarboxylate superplasticizer 50 parts
[0067] Sodium alkylbenzene sulfonate 3 parts
[0068] Sodium carboxymethyl cellulose 1 part
[0069] 3 parts calcium formate
[0070] Methanol 5 parts
[0071] 7 parts of triterpene saponins
[0072] Mass concentration is 15 parts of citric acid solution of 98%
[0073] 2 parts aluminum sulfate
[0075] 20 parts of water.
[0076] Wherein, the weight average molecular weight of the polycarboxylate water reducer is 15,000-80,000.
[0077] A preparation method of concrete water reducer, comprising the following steps:
[0078] (1) Add polycarboxylate water reducer, sodium alkylbenzene sulfonate, sodium carboxymethylcellulose, calcium formate, low molecular weight alcohol and aluminum sulfate in the reaction kettle in sequence, heat and stir to 60°C, Keep stirring for 30min;
[0079...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com