Anti-discoloration advertising material
An anti-discoloration and advertising technology, applied in the direction of anti-corrosion coatings, coatings, etc., can solve the problems of easy discoloration and deterioration, and unsatisfactory anti-discoloration effects, and achieve the effects of not easy to fade, conducive to popularization and application, and convenient production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0026] Further, the anti-discoloration advertising material is prepared by the following method:
[0027] a. Weigh the material, mix the inorganic pigment, acrylic resin, mannitol, sorbitol, and preservative;
[0028] b. Add slow-release agent to the mixture obtained in step a, mix well, then add wollastonite and alkylphenol polyoxyethylene ether, mix well, heat to 25-35°C and keep it warm for 20-25min to obtain the mixture;
[0029] c. mix polyethylene and polyacrylamide;
[0030] d. Calcium carbonate and ethyl cellulose are mixed;
[0031] e. Mix the mixed materials in steps c and d at 100-110°C for 5-8 minutes, add foaming agent, mix at 120-140°C for 8-12 minutes, cool to 80-85 °C, add the mixture obtained in step b, keep at 80-85 °C, 0.5-0.6Mpa for 15-20 minutes to obtain the anti-discoloration advertising material.
[0032] The process of the preparation method of anti-tarnish advertising material of the present invention is as follows:
[0033] a. Weigh the material,...
Embodiment 1
[0039] Take by weighing 100 parts by weight of polyethylene, 10 parts by weight of inorganic pigment iron oxide red, 12 parts by weight of acrylic resin, 6 parts by weight of mannitol, 18 parts by weight of wollastonite, 6 parts by weight of sorbitol, and 20 parts by weight of polyethylene glycol, 15 parts by weight of calcium carbonate, 6 parts by weight of polyacrylamide, 5 parts by weight of ethyl cellulose, 0.2 parts by weight of isothiazolinone, 0.15 parts by weight of alkylphenol polyoxyethylene ether, and 2 parts by weight of cyclopentane.
[0040] a. Mix the inorganic pigment iron oxide red, acrylic resin, mannitol, sorbitol, and isothiazolinone;
[0041] b. Add polyethylene glycol to the mixture obtained in step a, mix well, then add wollastonite and alkylphenol polyoxyethylene ether and mix well, heat to 30°C for 20min to obtain the mixture;
[0042] c. mix polyethylene and polyacrylamide;
[0043] d. Calcium carbonate and ethyl cellulose are mixed;
[0044] e. Mix...
Embodiment 2
[0046] Weigh 100 parts by weight of polyethylene, 10 parts by weight of inorganic pigment iron blue, 12 parts by weight of acrylic resin, 8 parts by weight of mannitol, 20 parts by weight of wollastonite, 8 parts by weight of sorbitol, 10 parts by weight of polyethylene glycol, hydroxy 15 parts by weight of methylcellulose, 20 parts by weight of calcium carbonate, 5 parts by weight of polyacrylamide, 4 parts by weight of ethyl cellulose, 0.12 parts by weight of isothiazolinone, 0.15 parts by weight of alkylphenol polyoxyethylene ether, isoamyl 1.5 parts by weight of alkane.
[0047] a. Mix the inorganic pigment iron blue, acrylic resin, mannitol, sorbitol, and isothiazolinone;
[0048] b. Add polyethylene glycol and hydroxymethyl cellulose to the mixture obtained in step a, mix well, then add wollastonite and alkylphenol polyoxyethylene ether, mix well, heat to 35°C and keep it warm for 20min to obtain the mixture;
[0049] c. mix polyethylene and polyacrylamide;
[0050] d....
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com