Water-based ink applied on paper printing
A water-based ink and paper-based technology, which is applied in the field of ink printing, can solve the problems of drying speed, gloss, water-resistant tinting strength and adhesion decrease, increase ink viscosity, reduce ink drying speed, etc., and achieve stable and improved performance. Drying speed, the effect of improving the overall performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] A water-based ink applied to paper printing, characterized in that it is made of the following components in parts by weight: 40 parts of modified acrylic resin, 15 parts of pigment, 1.5 parts of filler, 1.2 parts of dispersant, 1.0 parts of neutralizing agent 0.6 parts of anti-precipitation agent, 0.3 parts of defoamer, 0.2 parts of thickener, 30 parts of solvent;
[0018] The preparation method of described modified acrylic resin comprises the following steps:
[0019] (1) Prepare the following raw materials in parts by weight: 45 parts of methyl methacrylate, 35 parts of butyl acrylate, 30 parts of acrylic acid, 15 parts of polyvinyl butyral, 10 parts of hydroxypropyl acrylate, 7 parts of ammonium persulfate, 3 parts of sodium lauryl sulfate, 1.0 parts of OP-10, 0.5 parts of ferric chloride, 2.5 parts of boric acid, 1.5 parts of sodium bicarbonate, 2.0 parts of ammonia water, 80 parts of deionized water;
[0020] (2) Mix methyl methacrylate, butyl acrylate, acrylic ...
Embodiment 2
[0026] A water-based ink applied to paper printing, characterized in that it is made of the following components in parts by weight: 45 parts of modified acrylic resin, 20 parts of pigment, 1.6 parts of filler, 1.3 parts of dispersant, 1.1 parts of neutralizing agent 0.7 parts of anti-precipitation agent, 0.4 parts of defoamer, 0.3 parts of thickener, 35 parts of solvent;
[0027] The preparation method of described modified acrylic resin comprises the following steps:
[0028] (1) Prepare the following raw materials in parts by weight: 50 parts of methyl methacrylate, 40 parts of butyl acrylate, 32 parts of acrylic acid, 18 parts of polyvinyl butyral, 12 parts of hydroxypropyl acrylate, 8 parts of ammonium persulfate, 4 parts of sodium lauryl sulfate, 1.1 parts of OP-10, 0.6 parts of ferric chloride, 2.8 parts of boric acid, 1.8 parts of sodium bicarbonate, 2.5 parts of ammonia water, 85 parts of deionized water;
[0029] (2) Mix methyl methacrylate, butyl acrylate, acrylic ...
Embodiment 3
[0035] A water-based ink applied to paper printing, characterized in that it is made of the following components in parts by weight: 50 parts of modified acrylic resin, 25 parts of pigment, 1.8 parts of filler, 1.4 parts of dispersant, 1.2 parts of neutralizing agent 0.8 parts of anti-precipitation agent, 0.5 parts of defoamer, 0.4 parts of thickener, 40 parts of solvent;
[0036] The preparation method of described modified acrylic resin comprises the following steps:
[0037] (1) Prepare the following raw materials in parts by weight: 55 parts of methyl methacrylate, 45 parts of butyl acrylate, 35 parts of acrylic acid, 20 parts of polyvinyl butyral, 15 parts of hydroxypropyl acrylate, 10 parts of ammonium persulfate, 5 parts of sodium lauryl sulfate, 1.2 parts of OP-10, 0.8 parts of ferric chloride, 3.0 parts of boric acid, 2.0 parts of sodium bicarbonate, 3.0 parts of ammonia water, 90 parts of deionized water;
[0038](2) Mix methyl methacrylate, butyl acrylate, acrylic ...