Water-based carpentry paint filler and preparation method thereof

A water-based wood paint and filler technology, applied in the field of furniture paint, can solve the problems of large paint cost, labor cost, waste, and difficulty in filling and leveling water-based wood paint, so as to reduce the coating cost, improve the hardness of the paint film, and avoid paint The effect of membrane collapse

Inactive Publication Date: 2018-11-13
合肥科天环保节能科技有限公司 +1
View PDF1 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

This process needs to waste a lot of paint cost and labor cost to achieve the ideal coating effect
[0004] Therefore, it is necessary to develop a filler that solves the problem that deep conduit substrates are difficult to fill and level during wood paint construction, especially water-based wood paint, so as to reduce the material cost of the coating and the labor cost of furniture coating

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Water-based carpentry paint filler and preparation method thereof
  • Water-based carpentry paint filler and preparation method thereof
  • Water-based carpentry paint filler and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0048] A preparation method for water-based wood paint filler, comprising the following steps:

[0049] 1) Put 5 parts of water into the dispersion tank;

[0050] 2) Add 0.3 parts of cellulose, 0.3 parts of pigment and filler dispersant, and 0.3 parts of defoamer to the dispersion tank in turn at a speed of 500 to 800 rpm, and increase the stirring speed in the dispersion tank to 800 to 800 Stir at 1000 rpm for 15-20 minutes; then use 0.1 parts of pH additive to adjust the pH value of the mixture in the dispersion tank to 8, then add 8 parts of 800 to 800-1000 rpm stirring Mesh heavy calcium and 15 parts of talcum powder, after adding the powder, increase the stirring speed to 1000-1200 rpm, and continue to disperse at high speed for 20-30 minutes.

[0051] 3) Add 35 parts of polyurethane emulsion, 3 parts of film-forming aid, 2 parts of grinding aid, and 0.1 part of bactericide into the reactor, and continue stirring for 10 to 20 minutes;

[0052] 4) Finally, add 0.5 parts ...

Embodiment 2

[0055] A preparation method for water-based wood paint filler, comprising the following steps:

[0056] 1) Put 8 parts of water into the dispersion tank;

[0057]2) Add 0.5 parts of cellulose, 0.5 parts of pigment and filler dispersant, and 0.6 parts of defoamer to the dispersion tank in sequence at a speed of 500 to 800 rpm, and increase the stirring speed in the dispersion tank to 800 to 800 Stir at 1000 rpm for 15-20 minutes; then use 0.3 parts of pH additive to adjust the pH value of the mixture in the dispersion tank to 8, then add 12 parts of 800 Mesh heavy calcium and 28 parts of talcum powder, after adding the powder, increase the stirring speed to 1000-1200 rpm, and continue to disperse at high speed for 20-30 minutes.

[0058] 3) Add 45 parts of polyurethane emulsion, 5 parts of film-forming aid, 4 parts of grinding aid, and 0.3 part of fungicide into the dispersion tank, and continue stirring for 10 to 20 minutes;

[0059] 4) Finally, add 1.5 parts of thickener to...

Embodiment 3

[0062] A preparation method for water-based wood paint filler, comprising the following steps:

[0063] 1) Put 11 parts of water into the dispersion tank;

[0064] 2) Add 0.8 parts of cellulose, 1 part of pigment and filler dispersant, and 0.8 parts of defoamer to the dispersion tank in sequence at a speed of 500-800 rpm, and increase the stirring speed in the dispersion tank to 800-800 rpm. Stir at 1000 rpm for 15-20 minutes; then use 0.5 parts of pH additive to adjust the pH value of the mixture in the dispersion tank to 8, then add 20 parts of 800 Mesh heavy calcium and 35 parts of talcum powder, after adding the powder, increase the stirring speed to 1000-1200 rpm, and continue to disperse at high speed for 20-30 minutes.

[0065] 3) Add 50 parts of polyurethane emulsion, 8 parts of film-forming aid, 7 parts of grinding aid, and 0.5 part of bactericide into the reactor, and continue stirring for 10 to 20 minutes;

[0066] 4) Finally, add 2 parts of thickener to the dispe...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention provides a water-based carpentry paint filler. The filler comprises the following raw material components in parts by weight: 33-53 parts of polyurethane emulsion, 4-12 parts of water, 0.2-1 part of cellulose, 0.2-1 part of a pigment filler dispersant, 0.1-1 part of a defoaming agent, 0.1-0.5 part of a pH additive, 5-25 parts of 800-mesh ground calcium carbonate, 12-40 parts of talcum powder, 2.5-10 parts of a coalescing agent, 2-8 parts of a polishing additive, 0.1-0.5 part of a bactericide and 0.1-3 parts of a thickener. The water-based carpentry paint filler provided by the invention is a carpentry paint filler which is high in solid content and good in filling property, avoids later-period collapse, is good in polishing property, reduces paint construction times, and is low in formulation cost and convenient in construction.

Description

technical field [0001] The invention relates to the field of furniture paint, in particular to a water-based wood paint filler and a preparation method thereof. Background technique [0002] At present, the base materials used in furniture on the market are mainly solid wood and solid wood veneer to reflect the natural texture of the furniture. Especially the boards of broad-leaved forests have clear and beautiful textures and are loved by most consumers. However, the broad-leaved forest board has deep texture and ducts, while the water-based wood paint has low solid content, poor filling performance, low hardness, and poor sanding performance. During the construction of wood paint, it needs multiple spraying and sanding. Filling the texture and ducts requires a high cost of manpower and material resources. [0003] On the furniture board, first apply a transparent primer or sealing primer, then spray the first transparent primer and polish; then spray the second transpare...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C09D175/04C09D7/65C09D7/61C09D15/00
CPCC08K2003/265C09D7/61C09D7/65C09D15/00C09D175/04C08L1/284C08K3/26C08K3/34
Inventor 戴家兵陈瑞金荣光程世友奚霞
Owner 合肥科天环保节能科技有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products