Solar heat reflection heat-insulation thin film and preparation method thereof
A technology of solar heat and film, which is applied in the field of solar heat reflective heat insulation film and its preparation, can solve the problems of inconvenient food storage and transportation, affecting living comfort, inconvenience of industrial production, etc., and achieves simple and easy preparation method, excellent solar Heat reflection and heat insulation performance, low production cost effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] (1) Weigh 90kg polyvinyl chloride, 6kg rutile titanium dioxide, 6kg hollow glass microspheres, 4.5kg talcum powder, 3kg barium sulfate, 4.5kg ultrafine calcium powder, 6kg kaolin, 3kg stabilizer and 33kg plasticizer into Mix and stir in a high-speed mixer, the stirring speed is 1000r / min, and the stirring time is 30min.
[0024] (2) Add the above homogeneously mixed mixture into a two-roller mixer for kneading and processing at a processing temperature of 145-165°C until the mixture has good fluidity and the surface is smooth and free of cracks.
[0025] (3) The material is calendered with a calender at a calendering temperature of 160-210°C, then cooled and rolled up to produce a solar heat reflective heat-insulating film.
Embodiment 2
[0027] (1) Weigh 95kg of polyvinyl chloride, 3kg of rutile titanium dioxide, 9kg of hollow glass microspheres, 4.5kg of talcum powder, 3kg of barium sulfate, 4.5kg of ultrafine calcium powder, 6kg of kaolin, 2.4kg of stabilizer and 39kg of plasticizer and add Mix and stir in a high-speed mixer, the stirring speed is 1000r / min, and the stirring time is 30min.
[0028] (2) Add the above homogeneously mixed mixture into a two-roller mixer for kneading and processing at a processing temperature of 145-165°C until the mixture has good fluidity and the surface is smooth and free of cracks.
[0029] (3) The material is calendered with a calender at a calendering temperature of 160-210°C, then cooled and rolled up to produce a solar heat reflective heat-insulating film.
Embodiment 3
[0031] (1) Weigh 99kg polyvinyl chloride, 4.5kg rutile titanium dioxide, 3kg hollow glass microspheres, 6kg talcum powder, 4.5kg barium sulfate, 6kg ultrafine calcium powder, 6kg kaolin, 2.7kg stabilizer and 35kg plasticizer to add Mix and stir in a high-speed mixer, the stirring speed is 1000r / min, and the stirring time is 30min.
[0032] (2) Add the above homogeneously mixed mixture into a two-roller mixer for kneading and processing at a processing temperature of 145-165°C until the mixture has good fluidity and the surface is smooth and free of cracks.
[0033] (3) The material is calendered with a calender at a calendering temperature of 160-210°C, then cooled and rolled up to produce a solar heat reflective heat-insulating film.
[0034] To sum up, a large number of fillers with high reflectivity are added to the solar heat reflective and heat insulating film of the present invention, which can protect the sun in the visible light region and near infrared region, that is...
PUM
| Property | Measurement | Unit |
|---|---|---|