A kind of environment-friendly coal-water slurry and preparation method thereof
An environmentally friendly water and coal slurry technology, applied in the field of coal chemical industry, can solve the problems of high environmental hazards, refractory degradation, environmental hazards, etc., and achieve the effects of reducing production costs, improving stability, and saving consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0039] A kind of preparation method of environment-friendly coal-water slurry of the present invention, realizes by following steps:
[0040] (1) Add casing processing wastewater and inorganic alkali into the reaction tank, start stirring, and heat up;
[0041] (2) React for 1 to 5 hours when the temperature rises to 80°C to 120°C;
[0042] (2) Then add acrylic acid and its ester waste water and initiator, and control the temperature at 80°C to 100°C to react for 1 to 3 hours after the addition;
[0043] (4) Put the above-mentioned reaction product together with coal powder and dispersant into a rod mill and mix, grind ore for 5-10 minutes, then grind ore in a ball mill for 5-10 minutes, and discharge to obtain coal water slurry.
Embodiment 1
[0046] A kind of environment-friendly coal-water slurry of the present invention is made of the raw material components of following proportioning by weight:
[0047] Casing processing waste water 180 parts
[0048] Sodium hydroxide 0.6 parts
[0049] Acrylic acid and its ester wastewater 180 parts
[0050] Ammonium persulfate 0.02 parts
[0051] Lignite coal powder 637.88 parts
[0052] 1.5 parts of sodium naphthalenesulfonate formaldehyde condensate.
[0053] A kind of preparation method of environment-friendly coal-water slurry of the present invention, realizes by following steps:
[0054] (1) Add 180 parts of casing processing wastewater and 0.6 parts of sodium hydroxide into the reaction tank, start stirring, and heat up;
[0055] (2) React for 1.5 hours when the temperature rises to 85°C;
[0056] (2) Then add 180 parts of acrylic acid and its ester waste water and 0.02 parts of ammonium persulfate, and control the temperature at 90°C for 1.5 hours after the addit...
Embodiment 2
[0059] A kind of environment-friendly coal-water slurry of the present invention is made of the raw material components of following proportioning by weight:
[0060] Casing processing waste water 150 parts
[0061] Sodium hydroxide 1.5 parts
[0062] Acrylic acid and its ester wastewater 165 parts
[0063] Ammonium persulfate 0.03 part
[0064] Lignite coal powder 681.47 parts
[0065] 2 parts of sodium methylnaphthalenesulfonate formaldehyde condensate.
[0066] A kind of preparation method of environment-friendly coal-water slurry of the present invention, realizes by following steps:
[0067] (1) Add 150 parts of casing processing wastewater and 1.5 parts of sodium hydroxide into the reaction tank, start stirring, and heat up;
[0068] (2) React for 2 hours when the temperature rises to 98°C;
[0069] (2) Then add 165 parts of acrylic acid and its ester wastewater and 0.03 part of ammonium persulfate, and after the addition, control the temperature and react at 95°C ...