[0028] A preparation method for preparing the SBS water-based spray glue described in the above technical scheme, comprising the following steps:
[0029] STP1: Prepare aqueous solution: dissolve sodium dodecylbenzenesulfonate in deionized water for use;
[0030] STP2: Prepare the mixed solution: stir the aromatic environmental protection solvent and cyclohexane at room temperature to form a uniform mixed solution;
[0031] STP3: Then add SBS to the mixed solution made by STP2 and stir evenly, then add tackifying resin and stir until completely dissolved and become a uniform liquid;
[0032] STP4: Add kerosene emulsifier to the solution prepared by STP3 and stir evenly, then add the aqueous solution of STP1 and stir evenly.
[0033] The SBS is a styrene-butadiene block copolymerized elastomer.
[0034] The styrene-butadiene block copolymer elastomer is SBS1401.
[0035] The tackifying resin comprises three mixtures of rosin, rosin glycerin and tert-butylphenolic resin.
[...
Embodiment 1
[0038] Example 1: 15 parts of cyclohexane; 10 parts of aromatic environment-friendly solvent oil; 15 parts of SBS; 10 parts of tackifying resin; 50 parts of aqueous solution. Among them, the tackifying resin is: 1 part of rosin, 6 parts of rosin glyceride, and 3 parts of tert-butylphenolic resin. The aqueous solution is: 11 parts of sodium dodecylbenzenesulfonate and 39 parts of deionized water. When preparing,
[0039] STP1: Prepare the aqueous solution: dissolve 11 parts of sodium dodecylbenzenesulfonate in 39 parts of deionized water for use;
[0040] STP2: Prepare mixed solution: Stir 10 parts of aromatic environmental protection solvent and 15 parts of cyclohexane at room temperature to form a uniform mixed solution;
[0041] STP3: Then add 15 parts of SBS to the mixed solution made by STP2 and stir evenly, then add 1 part of rosin, 6 parts of rosin glyceride, and 3 parts of tert-butylphenolic resin and stir until completely dissolved and become a uniform liquid;
[00...
Embodiment 2
[0043] Example 2: 20 parts of cyclohexane; 15 parts of aromatic environment-friendly solvent oil; 10 parts of SBS; 15 parts of tackifying resin; 5 parts of kerosene emulsifier; 35 parts of aqueous solution. Wherein the tackifying resin is: 3 parts of rosin, 9 parts of rosin glyceride, and 3 parts of tert-butylphenolic resin. The aqueous solution is: 6 parts of sodium dodecylbenzenesulfonate and 29 parts of deionized water.
[0044] When preparing,
[0045] STP1: Prepare the aqueous solution: dissolve 6 parts of sodium dodecylbenzenesulfonate in 29 parts of deionized water for use;
[0046] STP2: Prepare mixed solution: Stir 15 parts of aromatic environmental protection solvent and 20 parts of cyclohexane at room temperature to form a uniform mixed solution;
[0047] STP3: Then add 10 parts of SBS to the mixed solution made by STP2 and stir evenly, then add 3 parts of rosin, 9 parts of rosin glyceride, and 3 parts of tert-butylphenolic resin and stir until completely dissolve...
PUM

Abstract
Description
Claims
Application Information

- R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com