A kind of aluminum-plastic panel production process
A production process and technology of aluminum-plastic panels, applied in the direction of layered products, other household appliances, chemical instruments and methods, etc., can solve the problems of increased labor intensity, low production efficiency, and low tensile strength, so as to reduce labor intensity, Effects of improving productivity and securing stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] Such as Figure 1-5 As shown, a production process of an aluminum-plastic panel, the production process of the aluminum-plastic panel specifically includes the following steps:
[0041] Mixing and stirring: put 100 parts by weight of polyethylene in a stirring tank in advance and stir at 100-120r / min for 3-5 minutes, then pour in 3 parts by weight of talcum powder, 2 parts by weight of calcium carbonate, 15 parts by weight of Barium sulfate, 1 weight part of non-halogen flame retardant and 1 weight part of defoamer are stirred in a stirred tank at 400-450r / min for 30-45 minutes to obtain a plastic mixture, and the plastic mixture is sucked by a vacuum suction machine into the hopper of the extruder;
[0042] Extrusion blank: the plastic mixture is sucked into the extruder barrel 1 through the feed port 2, the motor drive device 3 is started, and the motor drive device 3 drives the extrusion screw in the extruder barrel 1 to rotate, and the extruder barrel 1 The other ...
Embodiment 2
[0049] The specific steps of the production process of the aluminum-plastic panel are as follows:
[0050] Mixing and stirring: put 100 parts by weight of polyethylene in a stirring tank in advance and stir at 100-120r / min for 3-5 minutes, then pour in 8 parts by weight of talcum powder, 7 parts by weight of calcium carbonate, 20 parts by weight of Barium sulfate, 3 parts by weight of non-halogen flame retardant and 2 parts by weight of defoamer are stirred in a stirred tank at 400-450r / min for 30-45 minutes to obtain a plastic mixture, and the plastic mixture is sucked by a vacuum suction machine into the hopper of the extruder;
[0051] Extrusion blank: the plastic mixture is sucked into the extruder barrel 1 through the feed port 2, the motor drive device 3 is started, and the motor drive device 3 drives the extrusion screw in the extruder barrel 1 to rotate, and the extruder barrel 1 The other end is provided with a connecting pipe 6, and the connecting pipe 5 is provided...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com