Embodiment 1
[0032] A kind of preparation method of veneer for wooden floor, comprises the following steps:
[0033] (1) Substrate and panel sorting:
[0034] Select pineapple lattice wood sliced into boards, select the substrate and panel from it, wherein the warpage of the substrate is less than 1%, and the warpage of the panel is less than 0.8%, put the substrate and panel into the oven and bake until the moisture content is 6%;
[0035] (2) Configure the adhesive:
[0036] Adhesive comprises the raw material composition of following parts by weight:
[0037] Dehydrated urea-formaldehyde resin: 90 parts;
[0038] Polyvinyl acetate: 15 parts;
[0039] Titanate coupling agent: 1 part;
[0040] Chlorinated olefins: 0.5 parts;
[0041] Urea: 0.1 parts;
[0042] Ammonium chloride: 0.5 parts;
[0043] Flour: 10 parts;
[0044] Wherein the solid content of the dehydrated urea-formaldehyde resin is 50%, the viscosity is Iwata NK-2 cup viscosity 12s, the above raw materials are mixed a...
Embodiment 2
[0050] A kind of preparation method of veneer for wooden floor, comprises the following steps:
[0051] (1) Substrate and panel sorting:
[0052] Select disc bean wood sliced into boards, select the substrate and panel from it, wherein the warpage of the substrate is less than 1%, and the warpage of the panel is less than 0.8%, put the substrate and panel into the oven and bake until the moisture content is 9% ;
[0053] (2) Configure the adhesive:
[0054] Adhesive comprises the raw material composition of following parts by weight:
[0055] Dehydrated urea-formaldehyde resin: 95 parts;
[0056] Polyvinyl acetate: 20 parts;
[0057] Titanate coupling agent: 2 parts;
[0058] Chloroalkenes: 1 part;
[0059] Urea: 0.5 parts;
[0060] Ammonium sulfate: 1 part;
[0061] Soy flour: 15 parts;
[0062] Wherein the solid content of the dehydrated urea-formaldehyde resin is 55%, the viscosity is Iwata NK-2 cup viscosity 15s, the above raw materials are mixed and stirred unt...
Embodiment 3
[0068] A kind of preparation method of veneer for wooden floor, comprises the following steps:
[0069] (1) Substrate and panel sorting:
[0070] Select ash wood sliced into boards, select the substrate and panel from it, wherein the warpage of the substrate is less than 1%, and the warpage of the panel is less than 0.8%, put the substrate and panel into the oven and bake until the moisture content is 7%;
[0071] (2) Configure the adhesive:
[0072] Adhesive comprises the raw material composition of following parts by weight:
[0073] Dehydrated urea-formaldehyde resin: 93 parts;
[0074] Polyvinyl acetate: 16 parts;
[0075] Titanate coupling agent: 1.5 parts;
[0076] Chloroalkenes: 1 part;
[0077] Urea: 0.1 part;
[0078] Ammonium chloride: 0.6 parts;
[0079] Flour: 12 parts;
[0080] Titanium dioxide: 0.5 parts;
[0081]Wherein the solid content of the dehydrated urea-formaldehyde resin is 52%, the viscosity is Iwata NK-2 cup viscosity 13s, the above raw mate...
PUM
Property | Measurement | Unit |
---|---|---|
Bonding strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com