Paper-based functional material and preparation method thereof
A functional material, paper-based technology, applied in pulp raw material addition process, paper, papermaking and other directions, can solve the lack of research on deodorization of household paper-based materials, etc., to improve the deodorization rate, improve strength, dry and wet Strength-enhancing effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] (1) Take a certain amount of nanocellulose and mix it with deionized water to obtain a 0.01% (w / w) nanocellulose suspension;
[0025] (2) Weigh a certain amount of antibacterial agent and deionized water and mix evenly to obtain a 0.1% (w / w) transparent solution, add 1% (w / w) deodorant to the above solution, stir at room temperature for 10 minutes, and obtain an antibacterial deodorant finishing agent;
[0026] (3) Add 0.05% (w / w) wet strength agent to the pulp fiber, stir for 1min, then add nano-cellulose suspension and antibacterial and deodorant finishing agent, stir for 1min, mix well, after papermaking, pressing and drying , to obtain paper-based functional materials.
Embodiment 2
[0028] (1) Take a certain amount of nanocellulose and mix it with deionized water to obtain a 10% (w / w) nanocellulose suspension;
[0029] (2) Take a certain amount of antibacterial agent and deionized water and mix evenly to obtain a 15% (w / w) transparent solution, add 15% (w / w) deodorant to the above solution, stir at room temperature for 10 minutes, and obtain an antibacterial deodorant finishing agent;
[0030] (3) Add the antibacterial and deodorant finishing agent prepared above to the nanocellulose suspension, and mix evenly to obtain a composite finishing agent; spray one side of the paper, and place the sprayed paper in an 80° C. dryer for 5 minutes, A paper-based functional material is obtained.
Embodiment 3
[0032] (1) Take a certain amount of nanocellulose and mix it with deionized water to obtain a 15% (w / w) nanocellulose suspension;
[0033] (2) Take a certain amount of antibacterial agent and deionized water and mix evenly to obtain a 20% (w / w) transparent solution, add 20% (w / w) deodorant to the above solution, stir at room temperature for 40min, and obtain an antibacterial deodorant finishing agent;
[0034] (3) The antibacterial and deodorant finishing agent prepared above is added to the nanocellulose suspension, and mixed uniformly to obtain a composite finishing agent; the paper is sprayed, and the spraying is carried out twice. First, after spraying one side of the paper, place it in the Dry in a drying cylinder at 80°C until it is 80% dry. After standing for 30 minutes, spray the other side of the paper, and dry the sprayed paper at 110°C to obtain a paper-based functional material.
PUM

Abstract
Description
Claims
Application Information

- R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com